Sodium ion symmetrical battery and preparation method thereof

By composite modification of layered nanomanganese dioxide and using carbon coating and cerium doping technology, the conductivity and stability of electrode materials are solved, and the cycling and electrochemical performance of sodium ion symmetric batteries are significantly improved. Efficient sodium ion migration and charge utilization are achieved.

CN119008829APending Publication Date: 2024-11-22YANCHENG TEACHERS UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411091795.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The layered manganese dioxide electrode material has low ion and electron conductivity and poor structural stability in sodium ion symmetric batteries, resulting in poor cycling performance, limiting its practical application.

Method used

By composite modification of layered nanomanganese dioxide, carbon-covered active material, cerium doping and sodium titanium phosphate composite treatment is used to form carbon-covered active material, improving the structural stability and conductivity of the electrode material and enhancing sodium Ion migration capability.

Benefits of technology

The cyclic stability and electrochemical performance of the electrode material are significantly improved, and the capacity retention rate is above 90% after 200 charges and discharges, extending the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986786770000081
    Figure BDA0004986786770000081
Patent Text Reader

Abstract

The invention discloses a sodium ion symmetric battery and a preparation method thereof, and belongs to the technical field of sodium ion batteries, absolute ethyl alcohol, a carbon-coated active material, a conductive agent and a binder are uniformly mixed in proportion to obtain an electrode slurry, a current collector is coated with the electrode slurry for press molding to obtain an electrode material, and the electrode material is dried to obtain the sodium ion symmetric battery. And assembling the diaphragm, a pair of electrode materials and the electrolyte to obtain the sodium ion symmetric battery, layered nano-manganese dioxide is used as a matrix, the first charge-discharge capacity of an electrode material is improved through cerium doping, sodium ions can be promoted to be diffused in the electrode material through compounding of sodium titanium phosphate, an ion transmission path is shortened, polydopamine can be embedded into pores of sodium titanium phosphate composite manganese dioxide particles in the coating process, and through carbonization, the specific surface area of the electrode material is increased. The formed large-specific-surface-area carbon material can improve the overall conductivity of an electrode material, can play a role in supporting a carbon-coated active material structure, reduces structural damage caused by volume expansion and shrinkage in the charging and discharging process, and improves the cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium ion symmetrical battery and a preparation method thereof. Background Art

[0002] There are three different concepts in the battery field, namely monolithic battery, symmetrical battery and half-cell. Monolithic battery refers to an independent battery unit with simple structure and low cost. Half-cell is a test device used to study the performance of electrode materials, which only contains one electrode and electrolyte. Symmetrical battery has a symmetrical electrode structure, and its positive and negative electrode materials have the same or similar activities, high energy density and power density, long cycle life, and is widely used in new energy vehicles and energy storage fields.

[0003] Symmetrical sodium-ion batteries use sodium ions as charge carriers, and have a higher energy density than symmetric lithium-ion batteries. Aqueous sodium-ion batteries are an important component of aqueous electrochemical energy storage systems, and have the advantages of long cycle life and rapid charge and discharge. The performance of electrode materials affects the electrochemical performance of symmetrical batteries, and how to improve the energy density of electrode materials is now a research focus. Layered manganese dioxide has the advantages of low cost, environmental friendliness, and high theoretical capacity, but it also has problems such as low ionic and electronic conductivity, poor structural stability, and poor cycle performance, which hinders its practical application. Summary of the invention

[0004] The purpose of the present invention is to provide a sodium ion symmetrical battery, which improves the cycle performance of the sodium ion symmetrical battery using manganese dioxide electrode material by composite modification of layered nano manganese dioxide; the second purpose is to provide a preparation method of the sodium ion symmetrical battery.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A sodium ion symmetrical battery comprises an electrode material, a separator and an electrolyte.

[0007] Furthermore, the electrolyte is prepared by mixing sodium perchlorate, deionized water and acetonitrile in a mass ratio of 120:18-27:100-130.

[0008] Furthermore, the separator includes but is not limited to PP / PE / PP composite film.

[0009] A method for preparing a sodium ion symmetrical battery comprises the following steps:

[0010] Anhydrous ethanol, carbon-coated active material, conductive agent and binder are uniformly mixed in a mass ratio of 30-60:85-90:2-4:5-8 to obtain electrode slurry, the electrode slurry is coated on a current collector, and roll-formed at 60-70°C and a pressure of 10MPa to obtain an electrode material; a pair of electrode materials, a separator and an electrolyte are assembled to obtain a sodium ion symmetrical battery.

[0011] Furthermore, the conductive agent is any one of Ketjen black, carbon nanotubes and graphene.

[0012] Furthermore, the binder is any one of polyethylene, polyvinyl alcohol and polyvinylidene fluoride.

[0013] Furthermore, the current collector includes but is not limited to a titanium mesh, a nickel mesh and a stainless steel mesh.

[0014] Further, the carbon-coated active material is prepared by the following steps:

[0015] Step 1: adding a sodium hydroxide solution with a molar concentration of 5 mol / L and a manganese chloride solution with a molar concentration of 0.5 mol / L into a reactor and stirring and mixing, adding a potassium permanganate solution with a molar concentration of 0.2 mol / L into the reactor, stirring for 30-45 min at 300-500 r / min, then adding cerium acetate hydrate into the reactor and continuing to stir for 30-45 min, aging the mixture at 20-25° C. for 24 h, hydrothermally reacting at 150-160° C. for 22-26 h, cooling naturally, filtering, washing the filter cake with deionized water until the last washing solution is neutral, and vacuum drying at 60-80° C. to obtain cerium-doped manganese dioxide nanosheets;

[0016] Furthermore, the dosage ratio of the sodium hydroxide solution, the manganese chloride solution, the potassium permanganate solution and the cerium acetate hydrate is 40 mL: 20 mL: 40 mL: 6.2 g.

[0017] Step 2: adding cerium-doped manganese dioxide nanosheets and ethylene glycol to a reactor and ultrasonically dispersing for 10-15 minutes, adding sodium vanadate, citric acid, disodium hydrogen phosphate and deionized water to the reactor, stirring for 20-30 minutes at 350-500 r / min, then heating to 155-160° C. and stirring for 12-14 hours, centrifugally filtering, vacuum drying the filter cake at 60-80° C., and then transferring it to a tubular vacuum furnace, heating to 800-820° C. at a rate of 5° C. / min, and keeping warm for 10-12 hours to obtain sodium titanium phosphate composite manganese dioxide particles;

[0018] Furthermore, the dosage ratio of cerium-doped manganese dioxide nanosheets, ethylene glycol, sodium orthovanadate, citric acid, disodium hydrogen phosphate and deionized water is 0.05-0.06 g: 5-6 mL: 0.1 g: 0.31 g: 0.23 g: 5-6 mL.

[0019] Step 3: Add sodium titanium phosphate composite manganese dioxide particles and Tris-HCl buffer with a molar concentration of 10 mmol / L into a reactor and ultrasonically disperse for 20-30 minutes. The pH value of the Tris-HCl buffer is 8.5. Add dopamine hydrochloride to the reactor, stir and react at 25-30°C and 200-300 r / min for 6-8 hours, filter, wash the filter cake with deionized water 2-3 times, vacuum dry at 60-80°C, and then transfer to a tubular vacuum furnace. Under argon protection, heat to 800-820°C at a rate of 5°C / min, and keep warm for 2.5-3 hours to obtain a carbon-coated active material.

[0020] Furthermore, the dosage ratio of sodium titanium phosphate composite manganese dioxide particles, Tris-HCl buffer and dopamine hydrochloride is 0.05g:50mL:0.1-0.11g.

[0021] Beneficial effects of the present invention:

[0022] The sodium ion symmetrical battery of the present invention adopts composite modified carbon-coated active materials to prepare electrode materials. The assembled battery has good cycle performance. Through electrochemical testing of half cells, the capacity retention rate is above 90% after 200 charge and discharge cycles, and the cycle stability is good.

[0023] The carbon-coated active material is based on layered nano manganese dioxide. Cerium doping helps to improve its structural stability, increase the initial charge and discharge capacity of the electrode material, achieve a higher number of sodium ion migration, and improve the electrochemical performance of the electrode material. Cerium doping can also improve the stripping and dispersion of layered nano manganese dioxide, which helps the in-situ growth and coating of sodium titanium phosphate. The composite of sodium titanium phosphate helps to promote the diffusion of sodium ions in the electrode material, shorten the ion transmission path, and the formed three-dimensional space structure also helps to alleviate the volume change of the electrode material during the charge and discharge process.

[0024] During the coating process, polydopamine can be embedded in the pores of sodium titanium phosphate composite manganese dioxide particles. After carbonization, the formed carbon material with a large specific surface area can improve the overall conductivity of the electrode material, reduce the charge loss during the charging and discharging process, and can play a role in supporting the structure of the carbon-coated active material, reduce the structural damage caused by volume expansion and contraction during the charging and discharging process, and improve the structural stability and cycle stability of the carbon-coated active material. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] Example 1: This example provides a sodium ion symmetric battery, which is prepared by the following preparation method:

[0027] Step 1: Add 40L of 5mol / L sodium hydroxide solution and 20L of 0.5mol / L manganese chloride solution into a reactor and stir to mix, add 40L of 0.2mol / L potassium permanganate solution into the reactor, stir at 300r / min for 30min, then add 6.2kg of cerium acetate hydrate into the reactor and continue stirring for 30min, age the mixture at 20°C for 24h, hydrothermally react at 150°C for 22h, cool naturally, filter, wash the filter cake with deionized water until the last washing solution is neutral, and vacuum dry at 60°C to obtain cerium-doped manganese dioxide nanosheets.

[0028] Step 2: Add 50g of cerium-doped manganese dioxide nanosheets and 5L of ethylene glycol into a reactor and ultrasonically disperse for 10 minutes, add 100g of sodium vanadate, 310g of citric acid, 230g of disodium hydrogen phosphate and 5L of deionized water into the reactor, stir at 350r / min for 20min, then heat to 155°C and stir to react for 12h, centrifuge and filter, vacuum dry the filter cake at 60°C, then transfer to a tubular vacuum furnace, heat to 800°C at a rate of 5°C / min, and keep warm for 10h to obtain sodium titanium phosphate composite manganese dioxide particles.

[0029] Step 3: Add 50g of sodium titanium phosphate composite manganese dioxide particles and 50L of Tris-HCl buffer with a molar concentration of 10mmol / L into a reactor and ultrasonically disperse for 20min. The pH value of the Tris-HCl buffer is 8.5. Add 100g of dopamine hydrochloride into the reactor and stir the reaction at 25°C and 200r / min for 6h. Filter and wash the filter cake twice with deionized water. Dry it in a vacuum oven at 60°C and then transfer it to a tubular vacuum furnace. Under argon protection, heat it to 800°C at a rate of 5°C / min and keep it warm for 2.5h to obtain a carbon-coated active material.

[0030] Step 4: Mix sodium perchlorate, deionized water and acetonitrile in a mass ratio of 120:18:100 to prepare an electrolyte; mix anhydrous ethanol, carbon-coated active material, Ketjen black and polyethylene in a mass ratio of 30:85:2:5 to obtain an electrode slurry, use a titanium mesh as a current collector, coat the electrode slurry on the current collector, and roll-form it at 60°C and a pressure of 10MPa to obtain an electrode material; use a PP / PE / PP composite film as a diaphragm, assemble a pair of electrode materials, a diaphragm and an electrolyte to obtain a sodium ion symmetrical battery.

[0031] Example 2: This example provides a sodium ion symmetric battery, which is prepared by the following preparation method:

[0032] Step 1: Add 40L of 5mol / L sodium hydroxide solution and 20L of 0.5mol / L manganese chloride solution into a reactor and stir to mix, add 40L of 0.2mol / L potassium permanganate solution into the reactor, stir at 400r / min for 35min, then add 6.2kg of cerium acetate hydrate into the reactor and continue stirring for 35min, age the mixture at 22°C for 24h, hydrothermally react at 155°C for 24h, cool naturally, filter, wash the filter cake with deionized water until the last washing solution is neutral, and vacuum dry at 70°C to obtain cerium-doped manganese dioxide nanosheets.

[0033] Step 2: Add 55g of cerium-doped manganese dioxide nanosheets and 5.5L of ethylene glycol into a reactor and ultrasonically disperse for 12min, add 100g of sodium vanadate, 310g of citric acid, 230g of disodium hydrogen phosphate and 5.5L of deionized water into the reactor, stir at 400r / min for 25min, then heat to 158°C and stir to react for 13h, centrifuge and filter, vacuum dry the filter cake at 70°C, then transfer to a tubular vacuum furnace, heat to 810°C at a rate of 5°C / min, and keep warm for 11h to obtain sodium titanium phosphate composite manganese dioxide particles.

[0034] Step 3: Add 50g of sodium titanium phosphate composite manganese dioxide particles and 50L of Tris-HCl buffer with a molar concentration of 10mmol / L into a reactor and ultrasonically disperse for 25min. The pH value of the Tris-HCl buffer is 8.5. Add 105g of dopamine hydrochloride into the reactor and stir the reaction at 28°C and 250r / min for 7h. Filter and wash the filter cake twice with deionized water. Dry it in vacuum at 70°C and then transfer it to a tubular vacuum furnace. Under argon protection, heat it to 810°C at a rate of 5°C / min and keep it warm for 2.8h to obtain a carbon-coated active material.

[0035] Step 4: Mix sodium perchlorate, deionized water and acetonitrile in a mass ratio of 120:22.5:115 to prepare an electrolyte; mix anhydrous ethanol, carbon-coated active material, carbon nanotubes and polyvinyl alcohol in a mass ratio of 45:88:3:6.5 to obtain an electrode slurry, use a nickel mesh as a current collector, coat the electrode slurry on the current collector, and roll-form it at 65°C and a pressure of 10MPa to obtain an electrode material; use a PP / PE / PP composite film as a separator, assemble a pair of electrode materials, a separator and an electrolyte to obtain a sodium ion symmetrical battery.

[0036] Embodiment 3: This embodiment provides a sodium ion symmetric battery, which is prepared by the following preparation method:

[0037] Step 1: Add 40L of 5mol / L sodium hydroxide solution and 20L of 0.5mol / L manganese chloride solution into a reactor and stir to mix, add 40L of 0.2mol / L potassium permanganate solution into the reactor, stir at 500r / min for 45min, then add 6.2kg of cerium acetate hydrate into the reactor and continue stirring for 45min, age the mixture at 25°C for 24h, hydrothermally react at 160°C for 26h, cool naturally, filter, wash the filter cake with deionized water until the last washing solution is neutral, and vacuum dry at 80°C to obtain cerium-doped manganese dioxide nanosheets.

[0038] Step 2: Add 60g of cerium-doped manganese dioxide nanosheets and 6L of ethylene glycol into a reactor and ultrasonically disperse for 15 minutes, add 100g of sodium vanadate, 310g of citric acid, 230g of disodium hydrogen phosphate and 6L of deionized water into the reactor, stir at 500r / min for 30min, then heat to 160°C and stir to react for 14h, centrifuge and filter, vacuum dry the filter cake at 80°C, then transfer to a tubular vacuum furnace, heat to 820°C at a rate of 5°C / min, and keep warm for 12h to obtain sodium titanium phosphate composite manganese dioxide particles.

[0039] Step 3: Add 50g of sodium titanium phosphate composite manganese dioxide particles and 50L of Tris-HCl buffer with a molar concentration of 10mmol / L into a reactor and ultrasonically disperse for 30min. The pH value of the Tris-HCl buffer is 8.5. Add 110g of dopamine hydrochloride into the reactor and stir the reaction at 30°C and 300r / min for 8h. Filter and wash the filter cake with deionized water 3 times. Dry it in vacuum at 80°C and then transfer it to a tubular vacuum furnace. Under argon protection, heat it to 820°C at a rate of 5°C / min and keep it warm for 3h to obtain a carbon-coated active material.

[0040] Step 4: Mix sodium perchlorate, deionized water and acetonitrile in a mass ratio of 120:27:130 to prepare an electrolyte; mix anhydrous ethanol, carbon-coated active material, graphene and polyvinylidene fluoride in a mass ratio of 60:90:4:8 to obtain an electrode slurry, use a stainless steel mesh as a current collector, coat the electrode slurry on the current collector, and roll-form it at 70°C and a pressure of 10MPa to obtain an electrode material; use a PP / PE / PP composite film as a diaphragm, assemble a pair of electrode materials, diaphragms and electrolytes to obtain a sodium ion symmetrical battery.

[0041] Comparative Example 1: Based on Example 3, without going through step 3, the sodium titanium phosphate composite manganese dioxide particles in step 2 are directly used as the active material to replace the carbon-coated active material in step 3, and the other steps remain unchanged to prepare the electrode material and assemble it into a sodium ion symmetrical battery.

[0042] Comparative Example 2: Based on Example 3, cerium acetate hydrate was not added in step 1, and the other steps remained unchanged to prepare electrode materials and assemble them into a sodium ion symmetrical battery.

[0043] Comparative Example 3: Based on Example 3, layered manganese dioxide is prepared without adding cerium acetate hydrate in step 1, and the layered manganese dioxide is directly used as the active material to replace the carbon-coated active material in step 3. The other steps remain unchanged to prepare electrode materials and assemble into a sodium ion symmetrical battery.

[0044] Performance tests were carried out on Examples 1 to 3 and Comparative Examples 1 to 3, and the performance of different electrode materials was detected by assembling half-cells: a stainless steel mesh with a thickness of 0.2 mm was uniformly used as the current collector, and the thickness of the electrode material after roll forming was 0.6 mm. Different half-cell positive electrode samples were prepared, and commercially available PP / PE / PP composite film was used as the separator, commercially available graphite was used as the negative electrode material, and the electrolyte prepared in Example 3 was used to assemble CR2032 button batteries in an argon glove box.

[0045] At room temperature, the first charge was charged at 0.1C constant current, the charging voltage was limited to 4.5V, the first charge capacity and the first discharge capacity were recorded, the first coulomb efficiency was calculated, and then the charge and discharge were cycled 200 times under the conditions of 0.5C charging, 1C discharging and the charge and discharge voltage was limited to 2.5V, and the capacity retention rate of different button cells after 200 cycles was recorded to evaluate the cycle stability of electrode materials of different sodium ion symmetric batteries. The results are shown in Table 1:

[0046] Table 1

[0047]

[0048] It can be seen from Table 1 that compared with the use of a single layered nano manganese dioxide in Comparative Example 3, the first coulombic efficiency of the electrode material in Examples 1 to 3 is higher, indicating that the sodium ion symmetrical battery can fully utilize its capacity during use, with small charge loss, which helps to extend the service life of the sodium ion symmetrical battery, and after 200 charge and discharge cycles, the capacity retention rate of the button batteries in Examples 1 to 3 is above 90%, and the cycle stability is good.

[0049] Comparative Example 1 shows that by coating and carbonizing polydopamine, polydopamine can be embedded in the pores of sodium titanium phosphate composite manganese dioxide particles during the coating process, and the formed carbon material with a large specific surface area can improve the overall conductivity of the electrode material, reduce the charge loss during the charge and discharge process, and can play a supporting role, reduce the structural damage caused by volume expansion and contraction during the charge and discharge process, and improve the structural stability and cycle stability of the carbon-coated active material. Comparative Example 2 shows that cerium doping can increase the initial charge and discharge capacity of the electrode material and improve the electrochemical performance of the electrode material.

[0050] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0051] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a sodium ion symmetric battery, characterized in that: The steps include: Step 1: adding sodium titanium phosphate composite manganese dioxide particles and Tris-HCl buffer with a concentration of 10 mmol / L and a pH value of 8.5 into a reactor for ultrasonic dispersion for 20-30 min, adding dopamine hydrochloride, stirring at 25-30° C. and 200-300 r / min for reaction for 6-8 h, filtering, washing, vacuum drying, and then transferring to a tubular vacuum furnace, heating at 5° C. / min to 800-820° C. under argon protection, and keeping warm for 2.5-3 h to obtain a carbon-coated active material; Step 2: Evenly mix anhydrous ethanol, carbon-coated active material, conductive agent and binder in a mass ratio of 30-60:85-90:2-4:5-8 to obtain electrode slurry, apply the electrode slurry on the current collector, roll-form at 60-70°C and a pressure of 10MPa to obtain electrode material, assemble a diaphragm, a pair of electrode materials and an electrolyte to obtain a sodium ion symmetrical battery; The diaphragm is a PP / PE / PP composite film; the electrolyte is a mixture of sodium perchlorate, deionized water and acetonitrile in a mass ratio of 120:18-27:100-130.

2. The method for preparing a sodium ion symmetrical battery according to claim 1, characterized in that: The dosage ratio of the sodium titanium phosphate composite manganese dioxide particles, Tris-HCl buffer and dopamine hydrochloride is 0.05 g:50 mL:0.1-0.11 g.

3. The method for preparing a sodium ion symmetrical battery according to claim 1, characterized in that: The current collector is any one of a titanium mesh, a nickel mesh and a stainless steel mesh.

4. The method for preparing a sodium ion symmetric battery according to claim 1, characterized in that: The conductive agent is any one of Ketjen black, carbon nanotubes and graphene.

5. The method for preparing a sodium ion symmetric battery according to claim 1, characterized in that: The binder is any one of polyethylene, polyvinyl alcohol and polyvinylidene fluoride.

6. The method for preparing a sodium ion symmetric battery according to claim 1, characterized in that: The sodium titanium phosphate composite manganese dioxide particles are prepared by the following steps: Cerium-doped manganese dioxide nanosheets and ethylene glycol are added to a reactor and ultrasonically dispersed for 10-15 minutes. Sodium vanadate, citric acid, disodium hydrogen phosphate and deionized water are then added, stirred at 350-500 r / min for 20-30 minutes, heated to 155-160° C. and stirred for reaction for 12-14 hours, centrifuged and filtered, the filter cake is vacuum dried at 60-80° C., then transferred to a tubular vacuum furnace, heated to 800-820° C. at 5° C. / min, and kept warm for 10-12 hours to obtain sodium titanium phosphate composite manganese dioxide particles.

7. The method for preparing a sodium ion symmetric battery according to claim 6, characterized in that: The dosage ratio of the cerium-doped manganese dioxide nanosheets, ethylene glycol, sodium orthovanadate, citric acid, disodium hydrogen phosphate and deionized water is 0.05-0.06 g: 5-6 mL: 0.1 g: 0.31 g: 0.23 g: 5-6 mL.

8. The method for preparing a sodium ion symmetric battery according to claim 6, characterized in that: The cerium-doped manganese dioxide nanosheets are prepared by the following steps: A 5 mol / L sodium hydroxide solution and a 0.5 mol / L manganese chloride solution are added into a reaction kettle and stirred to mix, and then a 0.2 mol / L potassium permanganate solution is added, and stirred at 300-500 r / min for 30-45 min, cerium acetate hydrate is added and stirred for 30-45 min, aged at 20-25° C. for 24 h, hydrothermally reacted at 150-160° C. for 22-26 h, naturally cooled, filtered, washed, and vacuum dried to obtain cerium-doped manganese dioxide nanosheets.

9. The method for preparing a sodium ion symmetric battery according to claim 8, characterized in that: The dosage ratio of the sodium hydroxide solution, the manganese chloride solution, the potassium permanganate solution and the cerium acetate hydrate is 40 mL: 20 mL: 40 mL: 6.2 g.

10. A sodium ion symmetrical battery, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 9.