Method for improving hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst

The NiCo2S4 catalyst and magnesium hydride ball mill were prepared by hydrothermal method to form a composite material, which solved the problem of low hydrogen storage performance of magnesium hydride and achieved the effect of significantly improving hydrogen storage performance and kinetic performance.

CN118992971APending Publication Date: 2024-11-22GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202411054109.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high thermodynamic stability of magnesium hydride (MgH2) and slow dehydrogenation/hydrogenation kinetics seriously restrict its practical application.

Method used

The NiCo2S4 catalyst was prepared by hydrothermal method and mixed with MgH2 powder by ball milling to form MgH2-NiCo2S4 composite material to improve its hydrogen storage performance.

Benefits of technology

It significantly reduces the dehydrogenation starting temperature and activation energy of MgH2, improves the kinetic performance of hydrogen absorption and release, enhances the circulation performance, and the raw materials used are easy to obtain and cheap, and the experimental process is simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118992971A_ABST
    Figure CN118992971A_ABST
Patent Text Reader

Abstract

The invention relates to a method for improving the hydrogen storage performance of magnesium hydride based on a NiCo2S4 catalyst, and belongs to the technical field of hydrogen storage materials. The magnesium-based composite hydrogen storage material is prepared from magnesium hydride and a catalyst through a ball milling method, the catalyst is double transition metal sulfide NiCo2S4, and the method comprises the steps that nickel chloride hexahydrate, cobalt chloride hexahydrate and urea are dissolved in water according to the molar ratio of 1: 2: 6, and a NiCo precursor is obtained after hydrothermal treatment; the preparation method comprises the following steps: dispersing 0.5 g of a NiCo precursor in 40 mL of water, carrying out uniform ultrasonic dispersion, slowly dropwise adding 20 mL of a 0.02 M sodium sulfide solution into the NiCo precursor dispersion liquid, and carrying out hydrothermal treatment to obtain a double-transition metal sulfide NiCo2S4; and finally, carrying out ball milling on magnesium hydride and the catalyst according to different mass ratios to obtain the magnesium-based composite hydrogen storage material. The used raw materials are rich in source, the preparation process is simple, and the prepared magnesium-based composite hydrogen storage material is stable in structure and has excellent dynamic performance and cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen storage materials, and in particular relates to a method for improving the hydrogen storage performance of magnesium hydride based on a NiCo2S4 catalyst. Background Art

[0002] Hydrogen energy has attracted extensive attention from researchers due to its high calorific value, cleanliness and renewability. However, hydrogen storage technology is the main obstacle to the application of hydrogen energy. Magnesium hydride (MgH2) is considered to be a very promising solid hydrogen storage material due to its abundant sources, low cost, high hydrogen storage capacity (mass capacity: 7.6wt%, volume capacity: 110g / L) and good reversibility. Unfortunately, the high thermodynamic stability of MgH2 (ΔH=75KJ / mol) and slow dehydrogenation / hydrogenation kinetics have seriously restricted the practical application of MgH2.

[0003] So far, researchers have mainly improved the hydrogen storage performance of MgH2 by alloying, nano-sizing, adding catalysts and other methods. Among them, adding catalysts is considered to be one of the simple and effective strategies. Adding transition metals as catalysts can weaken the Mg-H bond, making MgH2 unstable, thereby improving its hydrogen storage performance. Many studies have shown that double transition metals can better improve the hydrogen storage performance of MgH2, and transition metal sulfides can be used as MgS catalysts in the process of hydrogen absorption and desorption. Therefore, the development of a double transition metal sulfide is of great significance to improving the hydrogen storage performance of MgH2. Summary of the invention

[0004] The purpose of the present invention is to propose a method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst, prepare NiCo2S4 catalyst by hydrothermal method, significantly improve the hydrogen storage performance of MgH2, and help promote the practical application of MgH2.

[0005] The method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst of the present invention comprises the following steps:

[0006] (1) Nickel chloride hexahydrate, cobalt chloride hexahydrate and urea were first dissolved in water at a molar ratio of 1:2:6. The solution was then transferred to a stainless steel autoclave with a Teflon liner and kept in an oven at 180°C for 12 hours. After washing and drying, a NiCo precursor was obtained.

[0007] (2) Disperse 0.5 g of NiCo precursor in 40 mL of water and disperse it evenly by ultrasonication. Stir 20 mL of 0.02 M sodium sulfide solution thoroughly and then slowly drip it into the NiCo precursor dispersion. Finally, transfer the mixture to a Teflon stainless steel autoclave, heat it at 180 ° C for 6 to 12 h, and wash and dry it to obtain the double transition metal sulfide NiCo2S4.

[0008] (3) The prepared double transition metal sulfide NiCo2S4 and MgH2 powder were ball milled at a mass ratio of 0.5:9.5, 1:9 and 1.5:8.5 for 5 to 10 hours, the vacuum ball mill was kept in an argon atmosphere, the ball-to-powder ratio was 120:1, the rotation speed was 400 to 600 rpm, and the ball mill was stopped for 10 minutes after every 20 minutes of rotation. For subsequent performance testing, the obtained MgH2-NiCo2S4 composite material was stored in a glove box filled with argon atmosphere.

[0009] The present invention has the following characteristics:

[0010] (1) Compared with the prior art, the raw materials used in the present invention are all industrially produced raw materials, which are easy to obtain and cheap.

[0011] (2) The experimental process is simple and the equipment is easy to operate.

[0012] (3) The synthesized hollow tubular NiCo2S4 significantly improves the hydrogen storage performance of MgH2. Analysis shows that the best effect on the hydrogen absorption and desorption performance of MgH2 is achieved when 10wt% NiCo2S4 catalyst is added. The dehydrogenation starting temperature of the MgH2-10 NiCo2S4 composite material is 203℃, and the dehydrogenation peak temperature is 339.2℃, which is much lower than the desorption temperature of MgH2.

[0013] (4) With the addition of NiCo2S4 catalyst, the kinetics of hydrogen absorption and desorption of MgH2 are greatly improved. For example, the MgH2-10NiCo2S4 composite material can release 3.68wt.% and 5.95wt.% H2 in 10 minutes at 275℃ and 300℃, and the dehydrogenation is basically completed within 5 minutes at 325℃, with the dehydrogenation amount reaching 6.11wt.% H2. In addition, at 75℃ and 100℃, the MgH2-10 NiCo2S4 composite material absorbs 1.01wt.% and 3.93wt.% H2 in 10 minutes, respectively. The MgH2-10NiCo2S4 composite material absorbs hydrogen rapidly at 150℃, and can absorb 5.54wt.% in 1 minute.

[0014] (5) The activation energy of the MgH2-10 NiCo2S4 composite material is 86.50±2.00 kJ / mol, which significantly reduces the dehydrogenation activation energy of MgH2. Moreover, the composite material has good cycle performance. After 10 cycles of hydrogen absorption and desorption, the dehydrogenation capacity retention rate is 98.80%. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is the XRD spectrum of NiCo2S4 in the embodiment of the present invention.

[0016] Figure 2 This is a SEM picture of NiCo2S4 in an embodiment of the present invention.

[0017] Figure 3 The TPD curve (a) and DSC curve (b) of the MgH2 and MgH2-10 NiCo2S4 composite materials in the embodiments of the present invention are shown.

[0018] Figure 4 Isothermal dehydrogenation curves of MgH2 and MgH2-10 NiCo2S4 composite materials at different temperatures in the embodiments of the present invention: (a) MgH2, (b) MgH2-10 NiCo2S4.

[0019] Figure 5 Arrhenius fitting curve diagram of MgH2 and MgH2-10 NiCo2S4 composite materials in embodiments of the present invention.

[0020] Figure 6 Isothermal hydrogen absorption curves of MgH2 and MgH2-10 NiCo2S4 composite materials at different temperatures in the embodiments of the present invention: (a) MgH2, (b) MgH2-10 NiCo2S4.

[0021] Figure 7 This is the isothermal dehydrogenation / hydrogenation cycle curve of the MgH2-10NiCo2S4 composite material at 300°C in an embodiment of the present invention.

[0022] Figure 8 This is the XRD spectrum of the MgH2-10NiCo2S4 composite material before and after cycling in the embodiment of the present invention. DETAILED DESCRIPTION

[0023] The specific implementation of the present invention is further described in detail below in conjunction with the embodiments and the accompanying drawings.

[0024] Example:

[0025] First, 2mmol nickel chloride hexahydrate, 4mmol cobalt chloride hexahydrate and 12mmol urea were dissolved in 60mL water and ultrasonicated for 15min. Then, the solution was transferred to a stainless steel autoclave with 100mL Teflon lining and kept in an oven at 180℃ for 12h. NiCo precursor was obtained. Then, 0.5g NiCo precursor was dispersed in 40mL water, ultrasonicated for 30min, 20mL 0.02M sodium sulfide solution was fully stirred, and then slowly dripped into the NiCo precursor dispersion, and finally the mixture was transferred to a 100mL Teflon stainless steel autoclave, heated at 180℃ for 8h, filtered with deionized water and ethanol, washed several times, and vacuum dried for 12h to obtain double transition metal sulfide NiCo2S4. The prepared NiCo2S4 and MgH2 powders were ball milled at a mass ratio of 1:9 for 6 hours, the vacuum ball mill was kept in an argon atmosphere, the ball-to-powder ratio was 120:1, the rotation speed was 500 rpm, and the ball mill was stopped for 10 minutes after every 20 minutes of rotation. For comparison, pure MgH2 powder was ball milled under the same conditions. For subsequent performance testing, the obtained MgH2 and MgH2-NiCo2S4 composites were stored in a glove box filled with argon atmosphere.

[0026] Firstly, the synthesized double transition metal sulfides were characterized by XRD and SEM. Figure 1 and Figure 2 The results showed that hollow nanotube NiCo2S4 catalysts with a length of 1-2 μm were successfully prepared.

[0027] In order to explore the effect of adding 10wt.% NiCo2S4 on the hydrogen storage performance of MgH2, the non-isothermal dehydrogenation performance and isothermal dehydrogenation performance of MgH2 and MgH2-10 NiCo2S4 composites were tested successively. Figure 3 (a) is the TPD curve of MgH2 and MgH2-10 NiCo2S4 composite materials, the heating rate is 2℃ / min. Figure 3 In (a), the initial dehydrogenation temperature of ball-milled MgH2 is 305℃, and the initial dehydrogenation temperature of MgH2-10 NiCo2S4 composite material is 203℃. The addition of NiCo2S4 catalyst reduces the initial dehydrogenation temperature of MgH2 by 102℃. Figure 3 (b) is the DSC curve of MgH2 and MgH2-10 NiCo2S4 composites, with a heating rate of 10℃ / min. It can be found that the endothermic peak temperature of ball-milled MgH2 is 402.5℃, and the endothermic peak temperature of MgH2-10 NiCo2S4 composite is 339.2℃, which is 63.3℃ lower than that of ball-milled MgH2. Figure 4It can be seen that the MgH2-10NiCo2S4 composite material can release 3.68wt.% and 5.95wt.% H2 at 275℃ and 300℃ for 10min, and the dehydrogenation is basically completed within 5min at 325℃, and the dehydrogenation amount reaches 6.11wt.% H2. However, at 300℃ and 325℃, MgH2 releases 0.094wt.% and 0.94wt.% H2 within 10min, respectively. From the Arrhenius fitting curve ( Figure 5 ) shows that the activation energy of MgH2 is 149.36±19.31 kJ / mol, while the activation energy of MgH2-10NiCo2S4 composite material is 86.50±2.00 kJ / mol. The results show that NiCo2S4 catalyst doping has a significant improvement on the dehydrogenation performance of MgH2.

[0028] In addition, isothermal hydrogen absorption tests were carried out on MgH2 and MgH2-10 NiCo2S4 composites. At 75°C and 100°C, the MgH2-10 NiCo2S4 composite absorbed 1.01wt.% and 3.93wt.% H2 within 10 minutes, respectively. The MgH2-10NiCo2S4 composite quickly absorbed hydrogen at 150°C, absorbing 5.54wt.% in 1 minute. However, at 150°C, MgH2 absorbed 2.04wt.% H2 within 10 minutes. The results show that the addition of catalysts can greatly improve the hydrogen absorption kinetics of the composites.

[0029] Figure 7 Isothermal dehydrogenation / hydrogenation cycle curve of MgH2-10 NiCo2S4 composite material at 300℃. Figure 7 As shown in the figure, the first dehydrogenation amount is 5.78wt.%, while the tenth dehydrogenation amount is 5.77wt.%, and the dehydrogenation capacity retention rate is 98.80%, indicating that the MgH2-10 NiCo2S4 composite material has good cycle performance. The XRD spectra of the MgH2-10 NiCo2S4 composite material before and after the cycle ( Figure 8 ) It can be seen that the synergistic effect between the in-situ generated multiphase catalytic systems MgS, Mg2Ni / Mg2NiH4 and Mg2Co / Mg2CoH5 significantly improved the hydrogen absorption and desorption kinetics of Mg / MgH2.

Claims

1. A method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst, characterized in that: The steps include: (1)(1) First, nickel chloride hexahydrate, cobalt chloride hexahydrate and urea are dissolved in water, and then the solution is transferred to a stainless steel autoclave with a Teflon liner and kept in an oven at 180°C for 12 hours. After washing and drying, the NiCo precursor is obtained. ; (2) Disperse 0.5 g of NiCo precursor in 40 mL of water, disperse evenly by ultrasonication, fully stir 20 mL of 0.02 M sodium sulfide solution, and then slowly drip into the NiCo precursor dispersion. Finally, transfer the mixture to a Teflon stainless steel autoclave, heat at 180°C for a certain period of time, wash and dry to obtain double transition metal sulfide NiCo2S4. ; (3) The prepared double transition metal sulfide NiCo2S4 and MgH2 powder were ball milled at different mass ratios for a period of time, and the vacuum ball mill was kept in an argon atmosphere. The ball-to-powder ratio was 120:

1. To prevent overheating, the ball mill was stopped for 10 minutes after every 20 minutes of rotation. For subsequent performance testing, the obtained MgH2-NiCo2S4 composite material was stored in a glove box filled with argon atmosphere.

2. A method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst according to claim 1, characterized in that: The molar ratio of the nickel chloride hexahydrate, the cobalt chloride hexahydrate and the urea is 1:2:

6.

3. A method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst according to claim 1, characterized in that: When the NiCo precursor is treated, it is heated at 180° C. for a certain time of 6 to 12 hours.

4. A method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst according to claim 1, characterized in that: The different mass ratios of NiCo2S4 and MgH2 powders are 0.5:9.5, 1:9 and 1.5:8.

5.

5. A method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst according to claim 1, characterized in that: The ball milling conditions include a ball milling time of 5 to 10 hours and a ball milling speed of 400 to 600 rpm.

6. A method for improving the hydrogen storage performance of magnesium hydride based on NiCo2S4 catalyst according to claim 1, characterized in that: The argon atmosphere is a glove box atmosphere filled with argon.

Citation Information

Patent Citations

  • Bimetal sulfide composite magnesium-based hydrogen storage material and preparation method thereof

    CN115159452A

Cited By

  • Preparation method and application of composite hydrogen storage material based on NiV2S4 and magnesium hydride

    CN119750663A

  • Preparation method and application of composite hydrogen storage material based on NiV2S4 and magnesium hydride

    CN119750663B

  • Synthesis method of nano magnesium metal and application of nano magnesium metal in hydrogen storage

    CN121315273A