Quick-drying early-strength fine aggregate concrete and preparation method thereof
By blending sulfoaluminate cement with ordinary silicate cement and matching it with appropriate aggregate materials, the problems of long concrete setting time and low early strength are solved, enabling the application of rapid setting and high-strength concrete, which is suitable for the construction of prefabricated buildings.
Patent Information
- Application Number
- CN202411081114.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
Existing concrete has a long setting time and low early strength, which cannot meet the construction requirements of prefabricated buildings that require no formwork and high compressive strength, especially in applications in confined spaces and areas with openings in the flanges of steel components.
The process involves blending sulfoaluminate cement with ordinary silicate cement, combining river sand of appropriate fineness and fine stone of appropriate particle size, accelerating concrete setting through hydration reaction, generating ettringite crystal skeleton to improve early strength, and adding expansion agent and high-efficiency water-reducing agent to improve construction performance.
It significantly shortens the concrete setting time, improves early and late strength, and enables the concrete to reach a compressive strength of over 20MPa within 24 hours and over 40MPa within 28 days, thereby enhancing construction efficiency and quality.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to a quick-drying early-strength fine-stone concrete and a preparation method thereof. Background Art
[0002] In conventional concrete construction of civil engineering projects, the initial setting time of ordinary concrete is about 4 to 10 hours. At this time, the early strength of concrete is only about 1.2MPa, or even lower. At this time, the concrete structure on the construction site cannot be demoulded, let alone withstand the design load.
[0003] Prefabricated buildings have the advantages of reducing the workload of wet work on site, greatly saving manpower and material resources, and greatly improving on-site construction efficiency. At the same time, there are many post-casting areas at the joints of components, which are the key parts for prefabricated components to form an integral connection. The traditional practice is to support the post-casting area with formwork and cast self-compacting concrete or grouting materials for filling, but there are many areas with narrow working space that are not convenient for formwork (such as the post-casting area of the PEC beam-column node), and it is necessary to open holes in the flanges of steel components (opening holes in the flanges will significantly reduce the bearing capacity of the steel structure). Therefore, the casting material needs to have the characteristics of no need for formwork, convenient construction, and high compressive strength, but the existing traditional materials cannot meet the above requirements.
[0004] For example, the invention patent with application publication number CN 113582624 A discloses a quick-drying early-strength concrete and its preparation method, wherein the raw materials for preparation include, by weight, 50-80 parts of silicate cement, 20-40 parts of silica fume, 30-45 parts of water, 35-45 parts of mineral powder, 100-130 parts of aggregate, 10-15 parts of polyvinyl alcohol, 0.05-0.3 parts of fumaric acid, 0.03-0.1 parts of montmorillonite, and 0.005-0.01 parts of admixture. However, the concrete prepared in this application takes a long time to solidify, which is not conducive to construction. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a quick-drying early-strength fine-stone concrete and a preparation method thereof. The prepared concrete has the characteristics of short setting time and high early strength.
[0006] The technical solution of the present invention to solve the above problems is as follows:
[0007] A quick-drying early-strength fine stone concrete comprises the following components in parts by weight: 195-330 parts of cement, 500-600 parts of sand, 100-300 parts of stone, 10-40 parts of expansion agent, 1-3 parts of water reducing agent and 80-145 parts of water.
[0008] Preferably, the cement is selected from at least one of sulphoaluminate cement and ordinary Portland cement.
[0009] Preferably, the weight ratio of the sulphoaluminate cement to ordinary Portland cement is (0.3-1):1.
[0010] Preferably, the strength grade of the sulphoaluminate cement is not less than 42.5; the strength grade of the ordinary Portland cement is not less than 42.5.
[0011] Ordinary Portland cement has low early strength and long setting time. Its main mineral components are tricalcium silicate, dicalcium silicate and tricalcium aluminate.
[0012] Sulphoaluminate cement is a kind of early strength cement, which is made by grinding limestone and bauxite as raw materials, anhydrous calcium sulphoaluminate and dicalcium silicate obtained by sintering as clinker with mixed materials (gypsum and limestone, etc.) as the main minerals.
[0013] The present application adopts compounding of sulphoaluminate cement and ordinary silicate cement, and the main components after compounding can be regarded as: tricalcium silicate, dicalcium silicate, tricalcium aluminate, anhydrous calcium sulphoaluminate. When the compound system encounters water and undergoes hydration reaction, the anhydrous calcium sulphoaluminate first hydrates to form aluminum gel and continues to react to form hydrated calcium sulphoaluminate (calcium sulfoaluminate), the dicalcium silicate is hydrated to form calcium hydroxide and hydrated calcium silicate, the tricalcium silicate is hydrated to form calcium hydroxide, and the calcium hydroxide will participate in the reaction of aluminum gel being converted into calcium sulfoaluminate, further accelerating the hydration process of anhydrous calcium sulphoaluminate, increasing the hydration rate, and sharply shortening the setting time of the system; at the same time, the consumption of calcium hydroxide can further promote the hydration rate of tricalcium silicate and further reduce the setting time.
[0014] Moreover, because the compounded tricalcium silicate promotes the hydration process of anhydrous calcium sulfoaluminate, the formation speed of ettringite is very fast, and it precipitates in the form of needles. The ettringite crystals intersect with each other in the concrete to form a crystalline skeleton, which rapidly increases the early strength of the concrete. At the same time, the aluminum gel generated in the hydration reaction fills the pores of the intersecting ettringite crystal skeleton, making the structure more compact, thereby improving the strength of the system; at the same time, because the hydration of tricalcium silicate is accelerated, the hardening speed of the concrete is further accelerated, thereby improving the strength of the concrete.
[0015] In addition, by compounding sulphoaluminate cement and ordinary Portland cement, a large amount of ettringite is generated in a short period of time and fills the pores in the concrete. The ettringite generated later directly provides effective expansion work, which reduces the shrinkage rate of concrete and avoids problems such as concrete slipping and sinking.
[0016] Preferably, the sand is medium river sand with a fineness modulus of 2.3 to 3.0, which complies with the provisions of "Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete" JGJ52. River sand can smoothly fill the gaps between fine stones and densely reinforce, which is conducive to improving the workability and construction performance of concrete.
[0017] Preferably, the stone is fine stone with a particle size of 5 to 16 mm, which complies with the provisions of "Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete" JGJ52. Adding 100 to 300 parts of fine stone with a particle size range of 5 to 16 mm is beneficial to the preparation and construction of the construction site, to the smooth filling of densely reinforced parts, and to the improvement of the construction performance and compactness of the concrete.
[0018] Preferably, the expansive agent comprises a UEA type expansive agent. The addition of the expansive agent can utilize the expansion property of the expansive agent during hardening to offset the shrinkage of the concrete.
[0019] Preferably, the water reducer comprises a polycarboxylic acid-based high-performance water reducer. Adding a high-efficiency water reducer can effectively reduce the amount of mixing water and improve the strength and compactness of concrete.
[0020] Preferably, the water is fresh water.
[0021] The present invention also provides a method for preparing the above-mentioned fast-drying early-strength fine-stone concrete, comprising the following steps:
[0022] S1. Mix the sand and stone in the formula amount to obtain a first mixture;
[0023] S2, adding the formulated amount of cement and expansion agent to the first mixture, stirring for 1 to 2 minutes, to obtain a second mixture;
[0024] S3. Mix the formulated amount of water reducer and water and add them to the second mixture. Stir for 1 to 3 minutes and then stop to obtain fast-drying and early-strength fine stone concrete.
[0025] The preparation method provided by the present invention is based on the characteristics of fast-drying and early-strength fine-stone concrete. The cementitious material and the admixture powder are first premixed to be evenly dispersed in the aggregate, and then the water reducer and water are evenly mixed and added at one time, so that the materials of the fast-drying and early-strength fine-stone concrete are fully mixed and evenly dispersed, a concrete mixture with the best performance is obtained, and fast-drying and early-strength is better achieved.
[0026] The present invention also provides the application of the quick-drying and early-strengthening fine-stone concrete, which can be applied to the fields of construction and civil engineering.
[0027] The present invention has the following beneficial effects:
[0028] (1) The present invention uses sulphoaluminate cement and ordinary silicate cement for compounding. The two interact with each other, shorten the setting time of concrete, and improve the early strength of concrete. The compressive strength of the prepared concrete after 24 hours of room temperature curing is greater than 20MPa; at the same time, the compounding of the two also improves the later strength of concrete. The 28-day compressive strength of the prepared concrete is greater than 40MPa, thereby increasing the application range of concrete;
[0029] (2) The concrete preparation method of the present invention is simple and easy to operate. During the preparation, the materials can be fully mixed and dispersed, so that the prepared concrete has good cohesiveness and filling properties, which helps to improve the construction efficiency and ensure the construction quality to the greatest extent;
[0030] (3) The raw material composition of the preparation of the present invention is simple, easy to obtain, low cost, and does not use admixtures, which is convenient for on-site construction. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in combination with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] A quick-drying early-strength fine stone concrete comprises the following components in parts by weight: 65 parts of sulphoaluminate cement, 130 parts of ordinary Portland cement, 500 parts of river sand with a fineness modulus of 2.3-3.0, 100 parts of fine stone with a particle size of 5-16 mm, 10 parts of an expansion agent, 3 parts of a water reducing agent and 80 parts of water.
[0034] The method for preparing the quick-drying early-strength fine-stone concrete comprises the following steps:
[0035] S1. Put the formulated amount of sand and stone into a mixer and mix them evenly to obtain a first mixture;
[0036] S2, adding the formulated amount of sulphoaluminate cement, ordinary Portland cement and expansion agent to the first mixture, stirring for 1 minute to obtain a second mixture;
[0037] S3. Mix the formulated amount of water reducer and water and add them to the second mixture. Stir for 2 minutes and then stop to obtain fast-drying and early-strength fine stone concrete.
[0038] Example 2
[0039] A quick-drying early-strength fine stone concrete comprises the following components in parts by weight: 75 parts of sulphoaluminate cement, 225 parts of ordinary Portland cement, 600 parts of river sand with a fineness modulus of 2.3-3.0, 300 parts of fine stone with a particle size of 5-16 mm, 40 parts of an expansion agent, 1 part of a water reducing agent and 145 parts of water.
[0040] The preparation method of the quick-drying and early-strength fine-stone concrete of this embodiment is the same as the preparation method in Example 1 except that the stirring time in S2 is 2 minutes.
[0041] Example 3
[0042] A quick-drying early-strength fine stone concrete comprises the following components in parts by weight: 100 parts of sulphoaluminate cement, 170 parts of ordinary Portland cement, 500 parts of river sand with a fineness modulus of 2.3-3.0, 200 parts of fine stone with a particle size of 5-16 mm, 25 parts of an expansion agent, 2 parts of a water reducing agent and 110 parts of water.
[0043] The preparation method of the quick-drying and early-strength fine-stone concrete in this embodiment is the same as the preparation method in Example 2.
[0044] Example 4
[0045] A quick-drying early-strength fine stone concrete comprises the following components in parts by weight: 130 parts of sulphoaluminate cement, 130 parts of ordinary Portland cement, 550 parts of river sand with a fineness modulus of 2.3-3.0, 180 parts of fine stone with a particle size of 5-16 mm, 30 parts of an expansion agent, 2 parts of a water reducing agent, and 105 parts of water.
[0046] The preparation method of the quick-drying and early-strength fine-stone concrete in this embodiment is the same as the preparation method in Example 2.
[0047] Comparative Example 1
[0048] A concrete comprises the following components in parts by weight: 260 parts of ordinary Portland cement, 550 parts of river sand with a fineness modulus of 2.3-3.0, 180 parts of fine stone with a particle size of 5-16 mm, 30 parts of an expansion agent, 2 parts of a water reducing agent, and 105 parts of water.
[0049] The preparation method of the concrete of this comparative example comprises the following steps:
[0050] S1. Put the formulated amount of sand and stone into a mixer and mix them evenly to obtain a first mixture;
[0051] S2, adding the formulated amount of ordinary Portland cement and expansion agent to the first mixture, stirring for 2 minutes, to obtain a second mixture;
[0052] S3. Mix the formulated amount of water reducer and water and add them to the second mixture. Stir for 2 minutes and then stop to obtain concrete.
[0053] Comparative Example 2
[0054] A concrete comprises the following components in parts by weight: 260 parts of sulphoaluminate cement, 550 parts of river sand with a fineness modulus of 2.3-3.0, 180 parts of fine stone with a particle size of 5-16 mm, 30 parts of an expansion agent, 2 parts of a water reducing agent, and 105 parts of water.
[0055] The preparation method of the concrete of this comparative example comprises the following steps:
[0056] S1. Put the formulated amount of sand and stone into a mixer and mix them evenly to obtain a first mixture;
[0057] S2, adding the formula amount of sulphoaluminate cement and expansion agent to the first mixture, stirring for 2 minutes, to obtain a second mixture;
[0058] S3. Mix the formulated amount of water reducer and water and add them to the second mixture. Stir for 2 minutes and then stop to obtain concrete.
[0059] Comparative Example 3
[0060] A concrete comprises the following components in parts by weight: 20 parts of sulphoaluminate cement, 190 parts of ordinary Portland cement, 550 parts of river sand with a fineness modulus of 2.3-3.0, 180 parts of fine stone with a particle size of 5-16 mm, 25 parts of an expansion agent, 2 parts of a water reducing agent, and 100 parts of water.
[0061] The preparation method of the concrete in this comparative example is the same as that in Example 2.
[0062] Comparative Example 4
[0063] A quick-drying early-strength fine stone concrete comprises the following components in parts by weight: 130 parts of sulphoaluminate cement, 130 parts of ordinary Portland cement, 550 parts of coarse river sand with a fineness modulus of 3.1-3.4, 180 parts of crushed stone with a particle size of 16-31.5 mm, 30 parts of an expansion agent, 2 parts of a water reducing agent, and 105 parts of water.
[0064] The preparation method of the concrete in this comparative example is the same as that in Example 2.
[0065] The concrete components of Examples 1 to 4 and Comparative Examples 1 to 4 are shown in the following table.
[0066] Table 1 Concrete components of Examples 1 to 4 and Comparative Examples 1 to 4
[0067]
[0068] The concretes prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were respectively tested according to GB / T50081-2016 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the test results are shown in the following table.
[0069] Table 2 Performance test data of concrete of Examples 1 to 4 and Comparative Examples 1 to 4
[0070] Final setting time (min) 24h compressive strength (MPa) 28d compressive strength (MPa) Example 1 60 26.3 45.3 Example 2 120 20.6 44.2 Example 3 50 27.2 50.4 Example 4 45 29 54.5 Comparative Example 1 232 14.1 39.9 Comparative Example 2 30 36.8 43.6 Comparative Example 3 191 19.1 36.2 Comparative Example 4 45 17.8 37.6
[0071] It can be seen from Table 1 and Table 2 that the final setting time of Examples 1 to 4 is shorter than that of Comparative Example 1, and the 24h compressive strength and 28d compressive strength are both greater than those of Comparative Example 1, indicating that compared with the use of ordinary Portland cement alone, the present invention compounding sulphoaluminate cement and ordinary Portland cement can significantly shorten the final setting time of concrete and improve the early strength and late strength of concrete; the setting time of Comparative Example 2 is shorter than that of Examples 1 to 4, and the open time is too short, which is not conducive to construction operation.
[0072] According to Table 1 and Table 2, it can be seen that the final setting time of Examples 1 to 4 is shorter than that of Comparative Example 3, and the 24h compressive strength and 28d compressive strength are both greater than those of Comparative Example 3, indicating that the addition ratio of sulphoaluminate cement in Comparative Example 3 is too small. The composite formula of the present invention can effectively shorten the final setting time of concrete and improve the early strength and late strength of concrete.
[0073] It can also be seen from Table 1 and Table 2 that the 24h compressive strength and 28d compressive strength of Examples 1 to 4 are greater than those of Comparative Example 4, indicating that the use of coarse river sand with a larger fineness modulus and crushed stone with a larger particle size cannot effectively fill the gaps between the raw materials, resulting in poor compactness of the concrete, which ultimately has a negative impact on the early strength and late strength of the concrete;
[0074] In summary, the method of the present invention compounds sulphoaluminate cement and ordinary Portland cement, and uses sand with a smaller fineness modulus and stone with a moderate particle size, so that the final setting time of the obtained concrete is significantly shortened, and the final setting time does not exceed 120 minutes. At the same time, the early strength and late strength of the concrete are improved, and the 24-hour compressive strength can reach more than 20MPa, and the 28-day compressive strength is greater than 40MPa.
Claims
1. A fast-drying, early-strengthening fine-stone concrete. It is characterized in that The invention comprises the following components in parts by weight: 195-330 parts of cement, 500-600 parts of sand, 100-300 parts of stone, 10-40 parts of expansion agent, 1-3 parts of water reducing agent and 80-145 parts of water.
2. The quick-drying, early-strength fine-stone concrete according to claim 1, It is characterized in that The cement is selected from at least one of sulphoaluminate cement and ordinary Portland cement.
3. The quick-drying, early-strength fine-stone concrete according to claim 2, It is characterized in that The weight ratio of the sulphoaluminate cement to ordinary Portland cement is (0.3-1):
1.
4. The quick-drying, early-strength fine-stone concrete according to claim 2, It is characterized in that The strength grade of the sulphoaluminate cement is not less than 42.5; the strength grade of the ordinary Portland cement is not less than 42.
5.
5. The quick-drying, early-strength fine-stone concrete according to claim 1, It is characterized in that The sand is medium river sand with a fineness modulus of 2.3 to 3.
0.
6. The quick-drying, early-strength fine-stone concrete according to claim 1, It is characterized in that The stone is fine stone with a particle size of 5 to 16 mm.
7. The quick-drying, early-strength fine-stone concrete according to claim 1, It is characterized in that The expansion agent includes a UEA type expansion agent.
8. The quick-drying, early-strength fine-stone concrete according to claim 1, It is characterized in that The water reducing agent includes a polycarboxylic acid-based high-performance water reducing agent.
9. A method for preparing a fast-drying, early-strength fine-stone concrete according to any one of claims 1 to 8, It is characterized in that The following steps are involved: S1. Mix the sand and stone in the formula amount to obtain a first mixture; S2, adding the formulated amount of cement and expansion agent to the first mixture, stirring for 1 to 2 minutes, to obtain a second mixture; S3. Mix the formulated amount of water reducer and water and add them to the second mixture. Stir for 1 to 3 minutes and then stop to obtain fast-drying and early-strength fine stone concrete.
10. Use of the quick-drying, early-strength fine-stone concrete according to any one of claims 1 to 8 in the fields of construction and civil engineering.
Citation Information
Patent Citations
Concrete for practical application of building industrial production
CN103964793A
Rapid-hardening and shrinkage-free concrete
CN107628795A
Super early strength concrete and preparation method thereof
CN112811876A
Steam-curing-free concrete for C40 prefabricated component and preparation method of steam-curing-free concrete
CN114195465A
A high early strength cement concrete composition having the self-healing for road pavement and a repairing method of road pavement using the same
KR101720034B1
Cited By
Phase change temperature adjusting wall and preparation method
CN120554071A
A phase change temperature regulating wall and a preparation method thereof
CN120554071B