A kind of low carbon thermally recycled aggregate shrinkage compensating concrete and preparation method thereof

By using mineral powder, fly ash, polypropylene fibers and composite expansion agents in concrete, the problem of easy cracks in concrete in ultra-long seamless structures is solved, the durability and crack resistance of concrete are improved, and the carbon is reduced emission.

CN116081995BActive Publication Date: 2024-11-19CHINA CONSTR WESTERN CONSTR NORTH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310033553.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-10
Publication Date
2024-11-19
Estimated Expiration
2043-01-10

AI Technical Summary

Technical Problem

Existing compensatory shrinkage concrete is prone to cracks in ultra-long seamless structures, mainly due to the hydration of gelled materials and the migration of moisture in the concrete, resulting in early deformation and cracks.

Method used

Use low-carbon thermal regenerated aggregate to compensate shrinkage concrete, improve the compactness of concrete by using the microagglomeration and morphological effects of ore powder and fly ash, add polypropylene fibers and composite expansion agents to control shrinkage and crack resistance, and reduce cement Use to reduce carbon emissions.

Benefits of technology

It significantly reduces the generation of cracks in concrete, improves the durability and crack resistance of concrete, and reduces carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004048301960000061
    Figure BDA0004048301960000061
  • Figure BDA0004048301960000071
    Figure BDA0004048301960000071
  • Figure BDA0004048301960000081
    Figure BDA0004048301960000081
Patent Text Reader

Abstract

The present application relates to a kind of low-carbon heat-regenerated aggregate compensating shrinkage concrete in the field of concrete, which includes the following components in parts by weight, 320 parts of cementitious materials, 300-350 parts of machine-made sand, 650-750 parts of recycled fine aggregate, 800-1000 parts of recycled coarse aggregate, 5-10 parts of water reducer, polypropylene fiber, composite expansion agent; the weight of the polypropylene fiber accounts for 0.8-1% of the weight of the cementitious material; the weight of the composite expansion agent accounts for 8-12% of the weight of the cementitious material. When preparing low-carbon heat-regenerated aggregate compensating shrinkage concrete, the following preparation steps are included, and machine-made sand, recycled fine aggregate, recycled coarse aggregate and water are mixed according to the ratio to prepare a premix; cement, fly ash, mineral powder, water reducer, polypropylene fiber and composite expansion agent are added to the premix according to the ratio and mixed for more than 120s, and low-carbon heat-regenerated aggregate compensating shrinkage concrete is obtained by uniform mixing. The present application has the effect of reducing cracks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of concrete, and in particular to a low-carbon thermally recycled aggregate shrinkage-compensated concrete and a preparation method thereof. Background Art

[0002] Shrinkage compensating concrete is a kind of micro-expansive concrete made by adding an appropriate amount of expansive agent to expansive cement or ordinary concrete. It can play a relatively compensatory effect on the shortcomings of ordinary concrete, such as large shrinkage deformation and easy cracking.

[0003] In recent years, the construction of various large-scale public buildings in my country has been booming, and the construction of airports in the northwest region has become a window of rapid development. For the concrete of general airport projects, its structure is generally an ultra-long seamless structure, and the quality of concrete molding is extremely important. In actual projects, more than 80% of concrete cracks are caused by the early deformation under non-load constraints. The hydration of cementitious materials and the migration of water in concrete are considered to be the main reasons for concrete shrinkage, which is also an important reason for the occurrence of concrete cracks.

[0004] The related art discloses a shrinkage compensating concrete, which includes the following raw material components in parts by weight: 296-340 parts of cement, 708-768 parts of medium sand, 1025-1050 parts of crushed stone, 30-45 parts of fly ash, 9.6-11.6 parts of admixture, 36-68 parts of expansion agent, and 150-160 parts of water; the water-cement ratio is 0.33-0.43.

[0005] When preparing the concrete disclosed in the above scheme, medium sand, crushed stone and water are stirred to obtain a premix; then cement, fly ash, expansion agent and the premix are mixed to obtain an intermediate mixture; finally, the admixture and the intermediate mixture are mixed to obtain cement mortar; the cement mortar is loaded into a mold, cast and formed, vibrated, and cured to obtain high-compensation shrinkage concrete.

[0006] With regard to the above-mentioned related technologies, the inventors believe that for concrete with ultra-long seamless structures, existing technical solutions mostly adopt the method of reducing the water-cement ratio of concrete to improve the crack resistance of concrete. However, the amount of cementitious material used is too large, and the hydration of cementitious material and the migration of water in concrete are also likely to cause shrinkage cracks in concrete. Summary of the invention

[0007] In order to improve the problem of cracks in shrinkage compensating concrete, the present application provides a low-carbon thermally recycled aggregate shrinkage compensating concrete and a preparation method thereof.

[0008] In the first aspect, the present application provides a low-carbon thermally recycled aggregate shrinkage-compensated concrete, which adopts the following technical scheme: 320 parts of cementitious material, 300-350 parts of machine-made sand, 650-750 parts of recycled fine aggregate, 800-1000 parts of recycled coarse aggregate, 5-10 parts of water reducer, 165 parts of water, polypropylene fiber, and composite expansion agent;

[0009] The cementitious material comprises the following components in weight: 150-180 parts of cement, 100-160 parts of fly ash, and 0-60 parts of mineral powder; the weight of the polypropylene fiber accounts for 0.8-1% of the weight of the cementitious material;

[0010] The weight of the composite expansion agent accounts for 8-12% of the weight of the gelling material.

[0011] By adopting the above technical scheme, the "micro-aggregate effect" and "morphological effect" of mineral powder and fly ash are used to improve the workability of concrete. After the mineral powder and fly ash are added, the particle size of the mineral powder and fly ash forms a particle size gradient with the particle size of cement particles, and the particles fill each other, thereby further reducing the gaps between the fine aggregate particles, making it more compact; and the moisture between the cement particles can be released to form free water to improve the fluidity of the concrete.

[0012] The fineness of mineral powder is higher than that of fly ash. After composite addition, the gaps between material particles are filled, and the component materials are tightly stacked, which further reduces the porosity, thereby increasing the density of the concrete structure and improving the durability of the concrete.

[0013] The composite concrete made of slag and fly ash replaces part of the cement in the concrete, which can increase the strength of the concrete, improve the working performance of the concrete, delay the setting time, reduce the temperature rise, reduce cracks and improve durability.

[0014] Finally, due to the large-scale use of slag and fly ash, the amount of cement used is reduced, which can significantly reduce the carbon emissions of concrete.

[0015] As green building materials, machine-made sand, recycled fine aggregate and recycled coarse aggregate also achieve the recycling of resources and will not affect the performance of concrete.

[0016] Adding polypropylene fiber can effectively control the micro cracks caused by factors such as shrinkage, drying shrinkage, temperature changes, etc. of concrete, inhibit the formation and development of cracks, and improve the concrete's crack resistance, impermeability, impact resistance and earthquake resistance.

[0017] The addition of composite expansive agent can make the concrete expand moderately, establish a certain prestress, offset the tensile stress generated by the concrete during the solidification and hardening process, and reduce the occurrence of cracks.

[0018] In this scheme, the use of fly ash, mineral powder, polypropylene fiber and composite expansion agent can synergistically improve the shrinkage crack problem of concrete by reducing the amount of cement and the use of admixtures. At the same time, the concrete materials use recycled aggregate, slag and fly ash, which is also greener.

[0019] Optionally, the composite expansion agent includes the following components in parts by weight: 5-10 parts of calcium sulfoaluminate, 30-35 parts of calcium oxide, 5-10 parts of magnesium oxide, 5-10 parts of alkali-treated bamboo fiber, 5-10 parts of zeolite powder, 5-10 parts of sodium citrate, and 3-5 parts of vermiculite powder.

[0020] By adopting the above technical scheme, the bonding strength between alkali-treated bamboo fiber and cement matrix is ​​improved, forming a stable three-dimensional network structure. At the same time, the fiber acts as a "bridge" between cement stone crystals, and the fiber and cement hydrate are tightly bonded to play a "tensioning" role.

[0021] The porous water absorption of zeolite powder can slow down the rate of humidity reduction inside the concrete, thereby increasing the hydration degree of magnesium oxide, thereby appropriately improving the expansion performance of magnesium oxide and improving the pore structure of the matrix.

[0022] Vermiculite powder can produce micro-expansion, has strong adsorption capacity, and can increase the strength of concrete.

[0023] Optionally, the alkali-treated bamboo fiber is obtained by soaking the bamboo fiber in 8%-10% by mass sodium hydroxide.

[0024] By adopting the above technical solution, bamboo fiber is a kind of cellulose extracted from bamboo, which has the advantages of low price, light weight, high specific strength and specific modulus. The bamboo fiber is treated with hydrogen oxidative modification, and the hemicellulose of the bamboo fiber reacts with -OH of the alkaline solution and is removed, while the lignin is not changed, and the fiber bundles of the main bamboo fiber are exposed and refined, so that the surface is improved, and the wettability and dispersibility of the bamboo fiber in cement slurry are improved.

[0025] Moreover, the combination of alkali-treated bamboo fiber and polypropylene fiber can enhance the crack resistance of concrete.

[0026] Optionally, the bamboo fiber is treated with sodium hydroxide and then mixed with carbon black, and the weight ratio of the bamboo fiber to the carbon black is (1-2):1.

[0027] By adopting the above technical scheme, the surface fiber bundles of bamboo fiber are exposed and refined after alkali treatment, and after mixing with carbon black, on the one hand, the dispersion uniformity of modified bamboo fiber can be increased, and on the other hand, the addition of carbon black can enhance the strength of bamboo fiber, thereby also enhancing the crack resistance of concrete.

[0028] Optionally, the bamboo fiber particle size is 80-100 mesh.

[0029] By adopting the above technical solution, the particle size of the bamboo fiber is selected within the above range, which has excellent dispersibility and can achieve the technical effect of increasing the crack resistance of concrete.

[0030] Optionally, the concrete components also include 2-3 parts of hydration heat inhibitor.

[0031] By adopting the above technical solution, the addition of hydration heat inhibitor can regulate the hydration process of C3S in cement, reduce the cement hydration rate in the accelerated period, reduce the early heat release of cement and delay the appearance time of temperature peak, and finally reduce the hydration temperature rise of concrete and the formation of concrete temperature cracks.

[0032] Optionally, the water is micro-nano bubble water.

[0033] By adopting the above technical solution, micro-nano bubble water is added to concrete, which can play the role of ball lubrication and increase the workability of concrete.

[0034] In a second aspect, the present application provides a method for preparing low-carbon thermally recycled aggregate shrinkage-compensated concrete, which adopts the following technical solution:

[0035] A method for preparing low-carbon thermally recycled aggregate shrinkage-compensated concrete comprises the following preparation steps:

[0036] Mixing machine-made sand, recycled fine aggregate, recycled coarse aggregate and water according to a proportion to prepare a premix;

[0037] Cement, fly ash, mineral powder, water reducing agent, polypropylene fiber and composite expansion agent are added into the premix according to the proportion and mixed for more than 120 seconds. Low-carbon thermally recycled aggregate shrinkage compensating concrete is obtained by mixing evenly.

[0038] By adopting the above technical solution, the preparation of concrete can be completed.

[0039] Optionally, a hydration heat inhibitor is also added during the preparation step.

[0040] By adopting the above technical solution, the addition of hydration heat inhibitor improves the hydration temperature in the preparation process and improves concrete cracks.

[0041] In summary, the present application includes at least one of the following beneficial technical effects:

[0042] 1. Slag and fly ash composite concrete replaces part of the cement in concrete, which can improve the strength of concrete, improve the working performance of concrete, delay the setting time, reduce temperature rise, reduce cracks and improve durability;

[0043] 2. The addition of composite expansion agent can make concrete expand moderately, establish a certain prestress, offset the tensile stress generated by concrete during the solidification and hardening process, and reduce the occurrence of cracks;

[0044] 3. The combination of alkali-treated bamboo fiber and carbon black increases the dispersion uniformity of bamboo fiber and improves the crack resistance of concrete; 4. The combination of alkali-treated bamboo fiber and polypropylene fiber can enhance the crack resistance of concrete. DETAILED DESCRIPTION

[0045] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples and comparative examples, they are carried out under conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can all be sourced from common commercial sources.

[0046] Cement: Commercially available ordinary Portland cement.

[0047] Fly ash: Secondary fly ash.

[0048] Mineral powder: S95 grade mineral powder.

[0049] Recycled fine aggregate: fineness modulus 2.5.

[0050] Preparation method of alkali-treated bamboo fiber

[0051] Preparation Example 1

[0052] 10 kg of bamboo fiber with a particle size of 80 mesh was soaked in 10% sodium hydroxide for 24 hours and dried at 105°C.

[0053] Preparation Example 2

[0054] 10 kg of bamboo fiber with a particle size of 100 meshes was soaked in 10% sodium hydroxide for 24 hours, the treated bamboo fiber was evenly mixed with 10 kg of carbon black, and then dried at 105°C.

[0055] Preparation Example 3

[0056] 10 kg of bamboo fiber with a particle size of 80 meshes was soaked in 10% sodium hydroxide for 24 hours, the treated bamboo fiber was evenly mixed with 5 kg of carbon black, and then dried at 105°C.

[0057] Preparation example of composite expansion agent

[0058] Preparation Example 4

[0059] 10 kg of calcium aluminum sulfate, 35 kg of calcium oxide and 5 kg of magnesium oxide were uniformly mixed to obtain a composite expansion agent.

[0060] Preparation Example 5

[0061] 7 kg of calcium aluminum sulfate, 32 kg of calcium oxide, and 7 kg of magnesium oxide were uniformly mixed to obtain a composite expansion agent.

[0062] Preparation Example 6

[0063] 5 kg of calcium aluminum sulfate, 30 kg of calcium oxide, and 10 kg of magnesium oxide were uniformly mixed to obtain a composite expansion agent.

[0064] Preparation Example 7

[0065] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 7kg of alkali-treated bamboo fiber, 7kg of zeolite powder, 7kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0066] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 1.

[0067] Preparation Example 8

[0068] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 5kg of alkali-treated bamboo fiber, 7kg of zeolite powder, 7kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0069] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 1.

[0070] Preparation Example 9

[0071] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 10kg of alkali-treated bamboo fiber, 7kg of zeolite powder, 7kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0072] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 1.

[0073] Preparation Example 10

[0074] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 7kg of alkali-treated bamboo fiber, 7kg of zeolite powder, 7kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0075] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 2.

[0076] Preparation Example 11

[0077] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 7kg of alkali-treated bamboo fiber, 7kg of zeolite powder, 7kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0078] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 3.

[0079] Preparation Example 12

[0080] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 7kg of alkali-treated bamboo fiber, 5kg of zeolite powder, 7kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0081] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 3.

[0082] Preparation Example 13

[0083] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 7kg of alkali-treated bamboo fiber, 10kg of zeolite powder, 7kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0084] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 3.

[0085] Preparation Example 14

[0086] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 7kg of alkali-treated bamboo fiber, 7kg of zeolite powder, 5kg of sodium citrate and 5kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0087] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 3.

[0088] Preparation Example 15

[0089] 7kg of calcium aluminum sulfate, 32kg of calcium oxide, 7kg of magnesium oxide, 7kg of alkali-treated bamboo fiber, 7kg of zeolite powder, 10kg of sodium citrate and 3kg of vermiculite are uniformly mixed to obtain a composite expansion agent.

[0090] The alkali-treated bamboo fiber adopts the material prepared in Preparation Example 3.

[0091] Table 1 Amount of each component of the composite expansion agent in Preparation Examples 4-9, 12-15

[0092]

[0093] Example 1

[0094] Low-carbon thermally recycled aggregate concrete includes the following components by weight: 160kg cement, 160kg fly ash, 300kg machine-made sand, 750kg recycled fine aggregate, 1000kg recycled coarse aggregate, 5kg water reducer, 2.56kg polypropylene fiber, and 25.6kg composite expansion agent.

[0095] The composite expansion agent is the composite expansion agent prepared in Preparation Example 4.

[0096] The method for preparing the low-carbon thermally recycled aggregate shrinkage-compensated concrete comprises the following steps: mixing machine-made sand, recycled fine aggregate, recycled coarse aggregate and water according to a proportion to prepare a premix;

[0097] Cement, fly ash, mineral powder, water reducing agent, polypropylene fiber and composite expansion agent are added into the premix according to the proportion and mixed for 120 seconds. Low-carbon thermally recycled aggregate shrinkage compensating concrete is obtained by mixing evenly.

[0098] Example 2

[0099] The difference between Example 2 and Example 1 lies in the different amounts of the components used and the fact that the composite expansion agent is the expansion agent prepared in Preparation Example 5.

[0100] Example 3

[0101] The difference between Example 3 and Example 1 lies in the different amounts of the components used and the fact that the composite expansion agent is the expansion agent prepared in Preparation Example 6.

[0102] Example 4

[0103] Low-carbon thermally recycled aggregate concrete includes the following components by weight: 160kg cement, 120kg fly ash, 40kg mineral powder, 310kg machine-made sand, 700kg recycled fine aggregate, 900kg recycled coarse aggregate, 8.5kg water reducer, 3kg polypropylene fiber, and 30kg composite expansion agent.

[0104] The composite expansion agent is the composite expansion agent prepared in Preparation Example 5. The water is micro-nano bubble water.

[0105] Example 5

[0106] The difference between Example 5 and Example 1 lies in the different amounts of the components used and the fact that the composite expansion agent is the expansion agent prepared in Preparation Example 7.

[0107] Example 6

[0108] The difference between Example 6 and Example 5 lies in the different amounts of the components of the cementitious material.

[0109] Example 7

[0110] The difference between Example 7 and Example 5 lies in the different amounts of the components of the gelling material.

[0111] Table 2 Concrete components of Examples 1-7

[0112]

[0113]

[0114] Experimental testing

[0115] 1. Compressive strength test: GB / T50081-2002 "Standard for experimental methods of mechanical properties of ordinary concrete" tests the mechanical properties of concrete.

[0116] 2. Test of limited expansion rate in water: Length measurement of specimen: Measure the initial length of the specimen within 1 hour after demoulding.

[0117] After measuring the initial length, the specimen is immediately placed in water for curing, and the length change in water after 7 days is measured, that is, the restricted expansion rate in water for 7 days.

[0118] After measuring the length of the specimen after curing in water for 7 days, put it into a constant temperature and humidity room (box) for curing for 14 days, and measure the length change, which is the limited expansion rate of 14 days in air.

[0119] Calculation of limited expansion rate: The limited expansion rate of the concrete under test shall be calculated according to the following formula:

[0120] E=(L1-L) / L0*100

[0121] Where: E-limited expansion rate (%);

[0122] L1-limited specimen length of the measured age (mm);

[0123] L- initial length of the limiting specimen (mm);

[0124] L0-limits the base length of the specimen, 140 mm.

[0125] The average value of the measurement values ​​of two similar specimens is taken as the measurement result of the limiting expansion rate, and the calculation should be accurate to 0.001mm.

[0126] Table 3 Experimental test results of Examples 1-7

[0127]

[0128] By analyzing the experimental results of Examples 1-3 and Example 4, it can be seen that when micro-nano bubble water is used as water, the strength of concrete can be improved to a certain extent. Therefore, the applicant can reasonably infer that the addition of nano bubble water will affect the dispersion properties of concrete, thereby promoting the hydration of cementitious materials to improve the strength of concrete.

[0129] Analyzing the experimental results of Examples 5-7, when the proportion of cementitious materials in concrete is adjusted, the strength of concrete will also be affected. Comparing Examples 5-7 with Examples 1-3, the combination of mineral powder, fly ash and cement is more effective in improving the strength of concrete, and the combination of the cementitious materials in Examples 5-7 with the composite expansion agent is more effective in improving the crack resistance of concrete.

[0130] Example 8

[0131] The difference between Example 8 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared in Preparation Example 8.

[0132] Example 9

[0133] The difference between Example 9 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared in Preparation Example 9.

[0134] Example 10

[0135] The difference between Example 10 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared in Preparation Example 10.

[0136] Embodiment 11

[0137] The difference between Example 11 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared in Preparation Example 11.

[0138] Example 12

[0139] The difference between Example 12 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared in Preparation Example 12.

[0140] Embodiment 13

[0141] The difference between Example 13 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared by Preparation Example 13.

[0142] Embodiment 14

[0143] The difference between Example 14 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared by Preparation Example 14.

[0144] Embodiment 15

[0145] The difference between Example 15 and Example 6 is that the composite expansion agent adopts the bamboo fiber prepared by Preparation Example 15.

[0146] Table 4 Concrete components of Examples 8-15

[0147]

[0148]

[0149] Examples 8-15 adopt the same detection method as Example 1.

[0150] Table 5 Experimental test results of Examples 8-15

[0151]

[0152] By analyzing Example 6, Example 8 and Example 9, when the amount of alkali-treated bamboo fiber in the composite expansion agent is adjusted, the strength and expansion rate of the concrete are affected. Therefore, the applicant can reasonably conclude that the alkali-treated fiber has a positive effect on the strength and crack resistance of the concrete.

[0153] Further analysis of Examples 10-11 shows that when the preparation method of the alkali-treated bamboo fiber is changed, the strength and crack resistance of the concrete are also improved. Therefore, it can be concluded that the alkali-treated bamboo fiber prepared in Preparation 10 and Preparation Example 11 has a higher improvement on the performance of concrete.

[0154] Finally, analyzing Examples 12-15, after the addition of zeolite powder, sodium citrate and vermiculite, the properties of the concrete changed to varying degrees, so the applicant can conclude that the performance of the composite expansive agent of the present application has a significant effect on improving the strength and crack resistance of concrete.

[0155] Example 16

[0156] The difference between Example 16 and Example 6 is that the components further include a hydration heat inhibitor.

[0157] When preparing concrete, the hydration heat inhibitor is added together with the composite expansion agent.

[0158] Embodiment 17

[0159] The difference between Example 17 and Example 6 is that the amount of hydration heat inhibitor used in the components is different.

[0160] When preparing concrete, the hydration heat inhibitor is added together with the composite expansion agent.

[0161] Embodiment 18

[0162] The difference between Example 18 and Example 6 is that the water in the component adopts micro-nano bubble water.

[0163] Embodiment 19

[0164] The difference between Example 19 and Example 6 is that the water in the components adopts micro-nano bubble water and also contains a hydration heat inhibitor.

[0165] When preparing concrete, the hydration heat inhibitor is added together with the composite expansion agent.

[0166] Table 6 Concrete components of Examples 16-19

[0167] Components Example 16 Embodiment 17 Embodiment 18 Embodiment 19 cement 160 160 160 160 Fly ash 120 120 120 120 Mineral powder 40 40 40 40 Machine-made sand 310 310 310 310 Recycled fine aggregate 700 700 700 700 Recycled coarse aggregate 900 900 900 900 Water reducing agent 8.5 8.5 8.5 8.5 water 165 165 165 165 Polypropylene fiber 3 3 3 3 Composite expansion agent 30 30 30 30

[0168] Table 7 Experimental test results of Examples 16-19

[0169] Test and Inspection Example 16 Embodiment 17 Embodiment 18 Embodiment 19 7d compressive strength / Mpa 21.8 21.6 22.5 22.9 28d compressive strength / Mpa 32 31.9 32.2 32.7 60d compressive strength / Mpa 35.4 35.8 35.9 36.2 7d limited expansion rate in water (%) 0.0026 0.0025 0.0025 0.0024 14d limited expansion rate in water (%) 0.0031 0.003 0.003 0.0029

[0170] By analyzing Examples 16 and 17, it can be concluded that after adding the hydration heat inhibitor, the strength and crack resistance of the concrete are improved.

[0171] In further comparison examples 18 and 19, when the water in the concrete is micro-nano bubble water and a hydration heat inhibitor is added, the strength and crack resistance of the concrete reach the best.

[0172] Comparative Example 1

[0173] The difference between Comparative Example 1 and Example 6 is that 320 kg of cement is used as the cementitious material in the components.

[0174] Comparative Example 2

[0175] The difference between Comparative Example 2 and Example 6 is that the components do not contain polypropylene fibers.

[0176] Comparative Example 3

[0177] The difference between Comparative Example 3 and Example 6 is that bamboo fiber is used in the composite expansion agent instead of alkali-treated bamboo fiber.

[0178] Comparative Example 4

[0179] The difference between Comparative Example 4 and Example 6 is that the composite expansion agent does not contain alkali-treated bamboo fiber.

[0180] Comparative Example 5

[0181] The difference between Comparative Example 5 and Example 6 is that the composite expansion agent does not contain alkali-treated bamboo fiber, and the concrete does not contain polypropylene fiber.

[0182] Comparative Example 6

[0183] The difference between Comparative Example 6 and Example 6 is that the composite expansion agent uses a common commercially available expansion agent. Table 8 Experimental test results of Comparative Examples 1-5

[0184] Test and Inspection Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 7d compressive strength / Mpa 16.8 17.2 19 18.7 16.2 18.6 28d compressive strength / Mpa 26.6 26.8 29.8 29.8 26.3 29.6 60d compressive strength / Mpa 28.1 28.6 32.7 32.8 27.7 32 7d limited expansion rate in water (%) 0.0043 0.0045 0.0034 0.0033 0.0048 0.0038 14d limited expansion rate in water (%) 0.005 0.0052 0.004 0.004 0.0055 0.0043

[0185] By analyzing Comparative Example 1 and Example 6, when cement is used as the cementitious material in the components, the strength of the concrete decreases and the expansion rate increases. Based on the above, it can be concluded that the composite concrete of slag and fly ash can improve the strength and crack resistance of the concrete.

[0186] Analysis of Comparative Example 2 and Example 6 shows that when the components do not contain polypropylene fibers, the strength of the concrete decreases and the expansion rate increases. Therefore, it can be concluded that polypropylene fibers can significantly increase the strength and reduce cracks in low-carbon thermally recycled aggregate shrinkage compensating concrete.

[0187] Further analysis of Example 3 shows that when bamboo fiber is used in the component instead of alkali-treated bamboo fiber, the strength of the concrete decreases and the expansion rate increases. Therefore, it can be concluded that the alkali-treated bamboo fiber has a greater impact on the performance of concrete when used in the composite expansion agent.

[0188] By analyzing comparative examples 3-6, it can be concluded that the alkali-treated expansion agent and the polypropylene fiber cooperate with each other to a certain extent to improve the crack resistance of the concrete. Specifically, the applicant speculates that the alkali-treated bamboo fiber and the polypropylene fiber can produce better cross-linking properties, thereby increasing the crack resistance of the concrete.

[0189] Finally, by analyzing the solutions of Comparative Example 6 and Example 6 of the present application, it can be clearly concluded that the composite expansion agent of the solution of the present application has a better performance improvement on the low-carbon thermally recycled aggregate shrinkage compensating concrete.

[0190] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A low-carbon thermally recycled aggregate shrinkage-compensated concrete, characterized in that: The invention comprises the following components in parts by weight: 320 parts of cementitious material, 300-350 parts of machine-made sand, 650-750 parts of recycled fine aggregate, 800-1000 parts of recycled coarse aggregate, 5-10 parts of water reducing agent, 165 parts of micro-nano bubble water, polypropylene fiber, composite expansion agent, and 2-3 parts of hydration heat inhibitor; The cementitious material comprises the following components in parts by weight: 150-180 parts of cement, 100-160 parts of fly ash, and 0-60 parts of mineral powder; The weight of the polypropylene fiber accounts for 0.8-1% of the weight of the gelling material; The weight of the composite expansion agent accounts for 8-12% of the weight of the gelling material; The composite expansion agent is composed of the following components in parts by weight: 5-10 parts of calcium sulfoaluminate, 30-35 parts of calcium oxide, 5-10 parts of magnesium oxide, 5-10 parts of alkali-treated bamboo fiber, 5-10 parts of zeolite powder, 5-10 parts of sodium citrate, and 3-5 parts of vermiculite. The alkali-treated bamboo fiber is obtained by soaking bamboo fiber in 8%-10% sodium hydroxide for 24 hours. The bamboo fiber is mixed with carbon black after being treated with sodium hydroxide. The weight ratio of the bamboo fiber to the carbon black is (1-2):

1. The particle size of the bamboo fiber is 80-100 meshes.

2. The method for preparing low-carbon thermally recycled aggregate shrinkage-compensated concrete according to claim 1, characterized in that: The method comprises the following preparation steps: mixing machine-made sand, recycled fine aggregate, recycled coarse aggregate and micro-nano bubble water according to a proportion to prepare a premix; adding cement, fly ash, mineral powder, water reducer, polypropylene fiber, composite expansion agent and hydration heat inhibitor into the premix according to a proportion and mixing for more than 120 seconds; and mixing evenly to obtain low-carbon heat-recycled aggregate shrinkage-compensated concrete.

Citation Information

Patent Citations

  • Low shrinkage, high strength cellular lightweight concrete

    CA2416493A1

  • Regeneration asphalt concrete and preparation method thereof

    CN109650824A

  • Recycled concrete and preparation method thereof

    CN111943575A

  • Nano bamboo fiber dry-mixed mortar with high tensile adhesive strength and preparation method of nano bamboo fiber dry-mixed mortar

    CN113943129A

  • Shrinkage-compensating self-compacting concrete and preparation method thereof

    CN114180890A