Ultrathin flexible glass as well as preparation method and application thereof
By adjusting the composition and preparation process of glass, the problem that ultra-thin flexible glass is difficult to have high strength and hardness in single molding is solved. The overflow pull-down method and chemical tempering treatment are used to achieve high transmittance and bending resistance. Thin flexible glass, suitable for flexible display equipment and other fields.
Patent Information
- Application Number
- CN202411109511.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-06
AI Technical Summary
It is difficult for existing ultra-thin flexible glass to have high strength, high hardness and high bending resistance during the primary molding process, and the secondary molding process has high cost and unenvironmental protection.
By adjusting the glass composition, it includes SiO2 50~70%, Al2O3 5~16%, Na2O 8~14%, K2O 2~6%, CaO 2~6%, MgO 2~6%, Li2O 0.1~2%, TiO2 0.1 ~2%, ZrO2 0.1~3%, is formed by overflow pull-down method in one go, and ball milling, melting, annealing and chemical tempering are performed during the preparation process to obtain ultra-thin with high transmittance, hardness and bending resistance. Flexible glass.
It has achieved high strength, high hardness and high bending resistance of ultra-thin flexible glass, with the ultimate bending radius ≤5mm, the maximum number of bending times ≥300,000 times, and the surface compressive stress is >850MPa, which is suitable for use in flexible display equipment and other fields.
Smart Images

Figure CN119080394A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of glass technology, and in particular to an ultra-thin flexible glass and a preparation method and application thereof. Background Art
[0002] Ultra-thin flexible glass (UTG) refers to flexible glass with a thickness of ≤0.1mm. It is a new material that combines the advantages of glass and plastic. It can not only be bent, but also has excellent hardness, transparency, heat resistance, and relatively stable mechanical and chemical properties. It not only plays a key role in flexible display fields such as folding mobile phones, flexible e-books, and curved TVs, but also has broad application prospects in flexible printing, space environment and other fields.
[0003] The preparation process of ultra-thin flexible glass is mainly divided into primary molding and secondary molding. The primary molding process mainly includes float method, overflow down-draw method and slit down-draw method. Its basic principle is to heat-draw the molten glass liquid into ultra-thin glass with a thickness of ≤0.1mm. The primary molding technology is extremely difficult, the raw materials are difficult to melt, and it is not easy to draw thin, so that the glass material cannot have high strength, high bending resistance and high hardness at the same time. The secondary molding process is to thin the thicker glass products. There are mainly physical thinning method, chemical thinning method and secondary down-draw method. Although the secondary molding process is simple, it has the disadvantages of high cost and environmental pollution.
[0004] Therefore, how to coordinate the strength, hardness and bending resistance of flexible glass from the perspective of glass composition has become the focus of research, and make it suitable for one-time molding into flexible glass by the overflow down-draw method. Summary of the invention
[0005] The purpose of the present invention is to provide an ultra-thin flexible glass and a preparation method and application thereof, wherein the ultra-thin flexible glass has high strength, high hardness and high bending resistance.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides an ultra-thin flexible glass, which comprises the following components, measured by mass percentage of oxides: SiO2 50~70%, Al2O3 5~16%, Na2O 8~14%, K2O 2~6%, CaO 2~6%, MgO 2~6%, Li2O 0.1~2%, TiO2 0.1~2%, and ZrO2 0.1~3%.
[0007] Optionally, the mass ratio of each component of the ultra-thin flexible glass meets the following conditions: 10% <Na2O+K2O+Li2O<18%;0.3%<TiO2+ZrO2<3%;5%<CaO+MgO<10%。
[0008] Optionally, when the thickness of the ultra-thin flexible glass is 0.05 mm, the transmittance in the visible light bands of 520 nm and 550 nm is >92%.
[0009] Optionally, the ultra-thin flexible glass has a Vickers hardness >560MPa, a maximum bending radius ≤5mm, and a maximum bending number ≥300,000 times.
[0010] Optionally, the surface compressive stress of the ultra-thin flexible glass is >850MPa.
[0011] A second aspect of the present invention provides a method for preparing ultra-thin flexible glass, the method comprising: The glass raw materials are ball-milled and mixed evenly, melted, formed and annealed, and cooled to room temperature to obtain flexible glass; the glass raw materials contain the following components: SiO2 50-70%, Al2O3 5-16%, Na2O 8-14%, K2O 2-6%, CaO 2-6%, MgO 2-6%, Li2O 0.1-2%, TiO2 0.1-2%, and ZrO2 0.1-3%; the flexible glass is thinned and chemically toughened.
[0012] Optionally, the ball milling speed is 300-500 r / min, and the time is 10-30 min.
[0013] Optionally, the melting temperature is 1600-1700° C., and the time is 2-5 h; the annealing temperature is 500-570° C., and the time is 0.5-1.5 h.
[0014] Optionally, the chemical tempering includes: chemically tempering the thinned flexible glass in a KNO3 molten salt at 400-420° C. for 1-3 hours.
[0015] A third aspect of the present invention provides an electronic display device, which includes the ultra-thin flexible glass provided by the first aspect of the present invention.
[0016] Through the above technical scheme, the present invention obtains an ultra-thin flexible glass by adjusting the composition design and preparation process of the ultra-thin flexible glass, which is suitable for one-time forming by the overflow down-draw method. The ultra-thin flexible glass not only has better strength and hardness, higher transmittance, but also has the characteristics of bending resistance. After chemical tempering, the maximum bending radius is ≤5mm, and the maximum bending number is ≥300,000 times.
[0017] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation to the present invention. In the accompanying drawings: Figure 1 It is a schematic diagram of the transmittance of the flexible glass in Embodiment 1 of the present invention. Specific Embodiments
[0019] The following provides a detailed description of the specific embodiments of the present invention in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not used to limit the present invention.
[0020] In the first aspect of the present invention, a kind of ultra-thin flexible glass is provided. Calculated by the mass percentage of oxides, the ultra-thin flexible glass comprises the following components: 50-70% of SiO2, 5-16% of Al2O3, 8-14% of Na2O, 2-6% of K2O, 2-6% of CaO, 2-6% of MgO, 0.1-2% of Li2O, 0.1-2% of TiO2, and 0.1-3% of ZrO2.
[0021] According to the present invention, optionally, the mass ratio between the components of the ultra-thin flexible glass satisfies the following conditions: 10% < Na2O + K2O + Li2O < 18%; 0.3% < TiO2 + ZrO2 < 3%; 5% < CaO + MgO < 10%. Through the above embodiments, the prepared flexible glass has better performance.
[0022] SiO2 is a glass network former and a necessary component for forming the glass skeleton. The higher its content, the more it can improve the chemical durability of the glass and the mechanical strength of the glass. However, as the content of SiO2 increases, the melting temperature and viscosity of the glass batch also increase, which not only leads to difficulties in melting the glass and increased energy consumption, but also is not conducive to thermoforming. If the content of SiO2 is too low, the glass structure is loose and prone to devitrification, which is not conducive to improving the chemical durability. In the present invention, the content of SiO2 being 50-70% can better balance the requirements in terms of glass component melting and mechanical strength.
[0023] Al2O3 is a commonly used glass network intermediate, which can effectively connect [SiO4] with the network modifiers, greatly improve the chemical stability of the glass, reduce the glass crystallization tendency, and at the same time can improve the glass hardness, impact strength, and elastic modulus. However, the melting point of Al2O3 is as high as 2045 °C, which increases the glass viscosity. Based on the current industrial melting conditions and capabilities, the content of Al2O3 in the present invention is preferably controlled at 5% - 16%, which can balance and coordinate the related physical and chemical properties and process properties such as the glass melting temperature, melting quality, forming temperature, glass crystallization, glass mechanical strength, and chemical stability.
[0024] R2O is the most important network exobody component and the material basis for ion exchange in glass. Alkali metal oxides (R2O) are mainly Li2O, Na2O and K2O, which can reduce the melting temperature of glass. The preferred content is 10%~18%. The coexistence of Li2O and Na2O can promote the secondary tempering of glass, making its ion exchange layer deeper and more impact resistant.
[0025] TiO2 is an intermediate oxide. In the glass structure, part of it is in the structural network as titanium oxide tetrahedron [TiO4], and part of it is outside the structure as titanium oxide octahedron [TiO6]. TiO2 can increase the refractive index and chemical stability of glass, and enhance the ability to absorb X-rays and ultraviolet rays. Its content is preferably 0.1~2%.
[0026] ZrO2 is an intermediate oxide that can improve the viscosity, hardness, elasticity, refractive index and chemical stability of glass and reduce the thermal expansion coefficient of glass. Its content should be between 0.1 and 3%.
[0027] According to the present invention, optionally, when the thickness of the ultra-thin flexible glass is 0.05 mm, the transmittance in the visible light bands of 520 nm and 550 nm is both greater than 92%.
[0028] According to the present invention, optionally, the ultra-thin flexible glass has a Vickers hardness >560 MPa, a maximum bending radius ≤5 mm, and a maximum bending number ≥300,000 times.
[0029] According to the present invention, optionally, the surface compressive stress of the ultra-thin flexible glass is >850MPa.
[0030] A second aspect of the present invention provides a method for preparing ultra-thin flexible glass, the method comprising: The glass raw materials are ball-milled and mixed evenly, melted, formed and annealed, and cooled to room temperature to obtain flexible glass; the glass raw materials contain the following components: SiO2 50-70%, Al2O3 5-16%, Na2O 8-14%, K2O 2-6%, CaO 2-6%, MgO 2-6%, Li2O 0.1-2%, TiO2 0.1-2%, and ZrO2 0.1-3%; the flexible glass is thinned and chemically toughened.
[0031] According to the present invention, optionally, the ball milling speed is 300-500 r / min, and the time is 10-30 min.
[0032] According to the present invention, optionally, the melting temperature is 1600-1700° C., and the time is 2-5 h; the annealing temperature is 500-570° C., and the time is 0.5-1.5 h.
[0033] According to the present invention, optionally, the chemical tempering comprises: chemically tempering the thinned flexible glass in a KNO3 molten salt at 400-420° C. for 1-3 hours.
[0034] A third aspect of the present invention provides an electronic display device, which includes the ultra-thin flexible glass provided by the first aspect of the present invention.
[0035] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0036] Examples 1-6 S1: Weigh the glass raw materials according to the ratio, and the glass raw materials and their ratios are shown in Table 1 and Table 2; after the glass raw materials are evenly mixed by ball milling, they are placed in a platinum crucible, and placed in a high-temperature lifting furnace to melt at 1650°C for 4 hours; the molten glass liquid is poured into a mold (preheated to 500°C) for casting, and then annealed according to the set temperature curve, the annealing temperature is 550°C, the time is 1 hour, and after cooling to room temperature, a flexible glass suitable for overflow down-draw production is obtained; S2: The flexible glass was thinned to a thickness of 0.05 mm and chemically toughened in a 410°C KNO3 molten salt for 2 h.
[0037] Comparative Examples 1-3 S1: Weigh the glass raw materials according to the ratio, and the glass raw materials and their ratios are shown in Table 1; after the glass raw materials are evenly mixed by ball milling, they are placed in a platinum crucible, and placed in a high-temperature lifting furnace to melt at 1650°C for 4 hours; the molten glass liquid is poured into a mold (preheated to 500°C) for casting, and then annealed according to the set temperature curve, the annealing temperature is 550°C, the time is 1 hour, and after cooling to room temperature, a flexible glass suitable for overflow down-draw production is obtained; S2: The flexible glass was thinned to a thickness of 0.05 mm and chemically toughened in a 410°C KNO3 molten salt for 2 h.
[0038] Test Examples 1-6 and Comparative Examples 1-3 The flexible glasses after chemical tempering in Examples 1-6 and Comparative Examples 1-3 were taken out and the surface molten salt was cleaned. The limit bending radius, number of bending times, surface compressive stress, transmittance, Vickers hardness, and elastic modulus were tested. The results are shown in Tables 1 and 2.
[0039] Transmittance: tested by UV-visible spectrophotometer.
[0040] Vickers hardness: measured using HXD-3000 Vickers hardness tester, with a loading force of 200g and a loading time of 15s Surface compressive stress: The test was conducted using the FSM-6000LE surface stress meter produced by Japan Orihara Industries Co., Ltd.
[0041] Limit bending radius and number of bending times: The test was carried out using the LT-UTG-SM-C flexible screen bending durability testing machine produced by Shenzhen Lvtu Precision Instrument Co., Ltd. at a bending speed of 200 times / min and a bending radius of 5mm.
[0042] Elastic modulus: The test was carried out using a PT-605BS four-point bending tester produced by Guangdong Beidou Precision Instrument Co., Ltd. at a speed of 10 mm / min.
[0043] Table 1
[0044] Table 2
[0045] The present invention obtains the ultra-thin flexible glass by adjusting the composition design and preparation process of the ultra-thin flexible glass. When the thickness of the ultra-thin flexible glass is 0.05 mm, the transmittance in the visible light bands of 520 nm and 550 nm is both greater than 92%, the surface compressive stress is greater than 850 MPa, the Vickers hardness is greater than 560 MPa, and after chemical tempering, the limit bending radius is ≤5 mm, and the maximum number of bending times is ≥300,000 times.
[0046] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0047] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0048] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. An ultra-thin flexible glass, characterized in that: Measured in percentage by mass of oxides, the ultra-thin flexible glass comprises the following components: SiO2 50-70%, Al2O3 5-16%, Na2O 8-14%, K2O 2-6%, CaO 2-6%, MgO 2-6%, Li2O 0.1-2%, TiO2 0.1-2%, and ZrO2 0.1-3%.
2. The ultra-thin flexible glass according to claim 1, wherein: The mass ratio of the components of the ultra-thin flexible glass meets the following conditions: 10% <Na2O+K2O+Li2O<18%; 0.3% <TiO2+ZrO2<3%; 5% <CaO+MgO<10%。 3. The ultra-thin flexible glass according to claim 1, wherein: When the thickness of the ultra-thin flexible glass is 0.05 mm, the transmittance in the visible light bands of 520 nm and 550 nm is greater than 92%.
4. The ultra-thin flexible glass according to claim 1, wherein: The ultra-thin flexible glass has a Vickers hardness of >560MPa, a maximum bending radius of ≤5mm, and a maximum bending number of ≥300,000 times.
5. The ultra-thin flexible glass according to claim 1, wherein: The surface compressive stress of the ultra-thin flexible glass is >850MPa.
6. A method for preparing ultra-thin flexible glass, characterized in that: The method includes: The glass raw materials are ball-milled and mixed uniformly, melted, molded and annealed, and cooled to room temperature to obtain flexible glass; the glass raw materials contain the following components: SiO2 50-70%, Al2O3 5-16%, Na2O 8-14%, K2O 2-6%, CaO 2-6%, MgO 2-6%, Li2O 0.1-2%, TiO2 0.1-2%, and ZrO2 0.1-3%; The flexible glass is thinned and chemically toughened.
7. The method according to claim 6, wherein: The ball milling speed is 300-500r / min, and the time is 10-30min.
8. The method according to claim 6, wherein: The melting temperature is 1600-1700°C and the time is 2-5h; The annealing temperature is 500-570° C., and the annealing time is 0.5-1.5 h.
9. The method according to claim 6, wherein: The chemical tempering includes: chemically tempering the thinned flexible glass in a KNO3 molten salt at 400-420° C. for 1-3 hours.
10. An electronic display device, characterized in that: The electronic display device comprises the ultra-thin flexible glass as described in any one of claims 1 to 5.
Citation Information
Patent Citations
High strength ultrathin float glass
CN102351420A
Silicate glass composition, ultra-thin glass made of same, preparing method and application
CN105384336A
Composition for glass, alumina silicate glass and preparation method and application of alumina silicate glass
CN106348588A
Alkali aluminosilicate flexible glass containing glass melt active material composition
CN111499188A
Ultrathin flexible tempered glass and preparation method thereof
CN117776519A
Cited By
Ultrathin glass, reinforced impact-resistant ultrathin glass and preparation method and application thereof
CN120271224A
Chemically tempered ultrathin flexible glass and preparation method thereof
CN120441193A
Chemically tempered ultra-thin flexible glass and method of making the same
CN120441193B
High-toughness ultrathin flexible glass and preparation method thereof
CN120903820A
A high-toughness ultrathin flexible glass and its preparation method
CN120903820B