Chitosan-acrylamide composite phenolic resin adhesive and application thereof

Through the use of chitosan-acrylamide composite phenolic resin adhesive, the problem of poor anti-mold effect of chitosan-copper complex anti-mold on different molds and insufficient anti-loss properties is solved, and a broad spectrum, Long-term anti-mold performance and improved internal bonding strength.

CN118995099APending Publication Date: 2024-11-22GUANGDONG ACAD OF FORESTRY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410979636.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Chitosan-copper complex anti-mold agent has uneven antibacterial properties for different types of molds and does not have long-term antibacterial properties, resulting in the inability to effectively prevent mildew when used in adhesives, especially for Aspergillus niger and T. green It has poor anti-mold effect and insufficient anti-lost property.

Method used

Using chitosan-acrylamide composite phenolic resin adhesive, the graft copolymer is formed by mixing the chitosan metal complex with the acrylamide solution, and combined with the phenolic resin adhesive, and is treated by vacuum and pressurized impregnation. , prepare recombinant or composite materials with broad-spectrum and long-acting anti-mold properties.

Benefits of technology

It achieves effective anti-mold for a variety of molds, improves the anti-lost property, and improves the internal glue strength of recombinant or composite materials, ensuring the anti-mold performance and mechanical strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995099A_ABST
    Figure CN118995099A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, and particularly discloses a chitosan-acrylamide composite phenolic resin adhesive and application thereof.The chitosan-acrylamide composite phenolic resin adhesive comprises a first component and a second component, the first component comprises a chitosan metal complex solution and an acrylamide solution which are mixed, and the second component comprises a phenolic resin adhesive. The chitosan-acrylamide composite phenolic resin adhesive disclosed by the invention has broad-spectrum and long-acting mildew-proof performance, and meanwhile, a recombinant or composite material prepared from the chitosan-acrylamide composite phenolic resin adhesive has improved internal bonding strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of adhesives, and specifically to a chitosan-acrylamide composite phenolic resin adhesive. The present application also relates to the application of the adhesive, especially in the preparation of reconstituted bamboo. Background Art

[0002] Chitosan is a natural high molecular organic compound with a broad-spectrum bactericidal effect and low toxicity, so it is widely used. However, the single use of chitosan on the material will reduce the mechanical strength of the material. Therefore, in reality, chitosan is mostly used as a mildew inhibitor in flexible materials. For example, a mildew-proof leather material added with chitosan is recorded in the invention patent application with publication number CN109673645A and the name "A method for preparing a new chitosan leather mildew-proof material", which is obtained by adding chitosan to the raw materials for preparing artificial leather and reacting them together. In building decoration materials, the loss of strength caused by the use of chitosan is unacceptable. Obviously, this defect of chitosan limits its application.

[0003] To overcome this problem, the prior art complexes chitosan with metal ions to obtain chitosan metal complexes. Compared with chitosan of a single component, chitosan metal complexes hardly affect the mechanical strength of the material, and also have improved mildew resistance and anti-loss performance. For example, the mildew-proof and anti-corrosion liquid recorded in the invention patent application with the publication number CN108714947A and the name "a method for impregnating a composite mildew-proof and anti-corrosion liquid-high temperature heat treatment of wood" includes a chitosan copper complex solution, a camphor leaf extract solution, a burdock leaf extract liquid, and a nano-titanium dioxide-Chinese herbal medicine composite anti-corrosion liquid. When used, the wood is immersed in the mildew-proof and anti-corrosion liquid, and the wood is impregnated with the mildew-proof and anti-corrosion liquid by a vacuum-pressure impregnation process, and then dried or subjected to high temperature heat treatment to obtain mildew-proof and anti-corrosion wood.

[0004] For the mildew-proof treatment of recombinant or composite materials, the prior art proposes to add chitosan-copper complex to adhesive to obtain mildew-proof adhesive, and use mildew-proof adhesive to glue to obtain mildew-proof recombinant or composite materials. For example, the patent for invention with the publication number CN102732196B, entitled "Environmentally friendly anticorrosive and mildew-proof phenolic adhesive and its production method", records a phenolic resin adhesive mixed with chitosan-copper, by separately preparing bisphenol A modified phenolic adhesive and anticorrosive and mildew-proof agent, and then mixing according to the ratio of (98-102): (1.5-2) to prepare a composite phenolic resin adhesive. When in use, only one dipping is required to complete the dipping treatment and the dipping anticorrosive and mildew-proof agent treatment, and a recombinant or composite material with anticorrosive and mildew-proof is obtained after pressing. Summary of the invention

[0005] The inventors have noticed that although chitosan-copper complex mildew inhibitors have broad-spectrum antibacterial properties, their antibacterial properties against different types of molds vary greatly. For example, chitosan-copper complex mildew inhibitors have a good mildew-proof effect against Penicillium citrinum (PC), but have a relatively poor mildew-proof effect against Aspergillius niger (AN) and Trichoderma viride (TV). In fact, they can be regarded as having no effective mildew-proof effect.

[0006] At the same time, although the chitosan-copper complex mildew inhibitor has improved anti-loss properties compared to the single-ingredient chitosan mildew inhibitor, it still cannot be considered to have long-lasting antibacterial properties.

[0007] It does not have universal and efficient antibacterial properties against molds, and does not have long-lasting antibacterial properties. These two problems also occur when used in combination with adhesives. In other words, the composite phenolic resin adhesive obtained by mixing the chitosan-copper complex mildew inhibitor with the phenolic resin adhesive will not improve its broad-spectrum properties. At the same time, in order to allow the chitosan-copper complex mildew inhibitor to be fully mixed with the phenolic resin adhesive, a water-based phenolic resin adhesive should be used. However, the treatment object, wood or bamboo, is a biomass material that is hydrophilic. From the results, the anti-loss property of the composite phenolic resin adhesive has not been further improved.

[0008] To this end, the first aspect of the present application proposes a chitosan-acrylamide composite phenolic resin adhesive, which specifically adopts the following technical solutions: The invention comprises a first component and a second component, wherein the first component comprises a mixed chitosan metal complex solution and an acrylamide solution, and the second component comprises a phenolic resin adhesive.

[0009] Preferably, the chitosan metal complex solution is a chitosan-copper solution.

[0010] As a further preference, the concentration of the chitosan metal complex solution is 2%-3%.

[0011] Preferably, the addition ratio of the first component to the second component is 1:(1-2.5).

[0012] Preferably, in the first component, the addition ratio of the chitosan metal complex solution to the acrylamide solution is 1:(0.5-2).

[0013] As a further preference, in the first component, the addition ratio of the chitosan metal complex solution and the acrylamide solution is 1:1.

[0014] Preferably, the first component is a graft copolymer solution of chitosan metal complex and acrylamide.

[0015] Preferably, the first component and the second component are pre-mixed.

[0016] The second aspect of the present application proposes an application of a chitosan-acrylamide composite phenolic resin adhesive, which specifically adopts the following technical scheme: At least the following steps are included: Step 1, immersing the material in the first component, first performing a vacuum impregnation treatment, then performing a pressure impregnation treatment, and finally performing a drying treatment to obtain a mildew-proof material; Step 2: immerse the anti-mildew material in the second component, first perform vacuum impregnation treatment, and then perform drying treatment to obtain the dipped anti-mildew material.

[0017] The third aspect of the present application proposes another scheme for the application of a chitosan-acrylamide composite phenolic resin adhesive, which specifically adopts the following technical scheme: The first component and the second component are mixed in proportion to obtain a composite phenolic resin adhesive, the material is immersed in the second component to obtain the composite phenolic resin adhesive, firstly a vacuum impregnation treatment is performed, then a pressure impregnation treatment is performed, and finally a drying treatment is performed to obtain an impregnated mildew-proof material.

[0018] In summary, the chitosan-acrylamide composite phenolic resin adhesive of the present application has a broad-spectrum and long-lasting mildew-proof performance. At the same time, the recombinant or composite material prepared using the chitosan-acrylamide composite phenolic resin adhesive has improved internal bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative labor.

[0020] Figure 1 (a) shows the microscopic morphology of chitosan-metal complexes. Figure 1 (b) shows the microscopic morphology of chitosan-metal complex grafted with acrylamide.

[0021] Figure 2 (a) (c) show the structure and morphology of starch in the cell wall of original bamboo. Figure 2 (e) shows the element contents of C, N, and O in starch in the cell wall of original bamboo. Figure 2(b) (d) show the structure and morphology of starch in the cell wall of bamboo after being treated with the first component. Figure 2 (f) shows the element contents of starch C, N, and O in the bamboo cell wall after treatment with the first component.

[0022] Figure 3 A comparison of pH values ​​of bamboo fibers is shown.

[0023] Figure 4 The results of the mildew resistance test of the recombinant bamboo of Example 2, Example 5, and Comparative Examples 1-3 with a period of 28 days are shown.

[0024] Figure 5 The anti-mildew test results of the recombinant bamboo of Example 2, Example 5, and Comparative Examples 1-3 after the anti-loss experiment with a period of 28 days are shown. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to better understand the technical solutions in the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.

[0026] The present application provides a chitosan-acrylamide composite phenolic resin adhesive, which comprises a first component and a second component, wherein the first component comprises a mixed chitosan metal complex solution and an acrylamide solution, and the second component comprises a phenolic resin adhesive.

[0027] By adding acrylamide solution, the chitosan-acrylamide composite phenolic resin adhesive of this embodiment: (1) has improved broad spectrum, has good mildew resistance against various molds, and the mildew resistance level of the prepared recombinant or composite material against various molds is 0; (2) has improved anti-loss property, and can be regarded as having long-lasting mildew resistance. After the anti-loss test, the mildew resistance level of the prepared recombinant or composite material against various molds is still 0; (3) The addition of acrylamide can promote the penetration of phenolic resin adhesive, and the prepared recombinant or composite material has higher internal bonding strength.

[0028] Specifically, wood and bamboo fiber cells contain a certain amount of starch. For example, the starch content in bamboo fiber cells reaches 2%-6%. Figure 1 As shown, after adding acrylamide into the chitosan-metal complex, acrylamide and chitosan formed a graft copolymer. Figure 1The microscopic morphology of chitosan-metal complex and the microscopic morphology after grafting acrylamide are shown in FIG. Therefore, chitosan-metal complex and acrylamide are not mixed relatively independently, and in fact the first component is a solution of graft copolymer of chitosan-metal complex and acrylamide.

[0029] Based on the above, in the first aspect, the first component can be coated alone or together with the second component on the starch surface in the cell wall of wood or bamboo, blocking the contact between mold and starch (nutrients), thereby blocking the growth of mold and preventing the spread of mold. Figure 2 As shown, the first component can change the structure and morphology of starch. Figure 2 The structure, morphology and C, N, O element contents of starch in the original bamboo cell wall, as well as the structure, morphology and C, N, O element contents of starch in the bamboo cell wall after being treated with the first component are shown in the figure. It can be seen that the starch structure and morphology have shrunk and collapsed, and the C and N contents are significantly reduced. This further destroys the necessary nutritional environment for mold growth, so that the first component of this embodiment alone or together with the second component has relatively good anti-mildew performance.

[0030] In a second aspect, the first component alone or in combination with the second component is capable of changing the pH of wood or bamboo fibers. Figure 3 As shown, taking bamboo fiber as an example, the pH value of the original bamboo fiber is 5.6, the pH value of the carbonized bamboo fiber is 6.0, and the pH value of the original bamboo fiber after being impregnated with chitosan-copper complex mildew inhibitor is 3.7. It is known that the pH value of the suitable environment for mold growth and reproduction is 4-6, so both the original bamboo and the carbonized bamboo have become moldy, and although the pH value of the original bamboo fiber impregnated with chitosan-copper complex mildew inhibitor has dropped to 3.7, it is still in the vicinity of the suitable range. The pH value of the original bamboo fiber impregnated with the first component or the mixed solution of the first component and the second component rises to 7.3, and the pH value of the carbonized bamboo fiber impregnated with the first component or the mixed solution of the first component and the second component rises to 7.2. Obviously, the first component can make the pH value of the wood or bamboo fiber away from the suitable pH range of mold alone or together with the second component, so that the environmental pH value of the wood or bamboo fiber is not conducive to the survival and growth of mold.

[0031] Through the above two aspects, since starch and appropriate pH value are essential nutrients and necessary environmental conditions for the survival and growth of various molds, by blocking the contact between molds and starch, changing the structure and morphology of starch, and making the pH value of wood or bamboo fiber far away from the pH value range suitable for molds, the survival, growth, spread and reproduction of molds can be fundamentally prevented to achieve a mildew-proof effect, and this mildew-proof effect is obviously applicable to a variety of molds, thereby expanding the broad spectrum of the first component of this embodiment alone or together with the second component.

[0032] When the first component permeates alone, the second component that permeates and solidifies can cover the first component to prevent it from being lost; when the first component and the second component are mixed and permeated, the first component is evenly dispersed in the second component, so the solidified second component can respectively cover the particles of the first component. At the same time, due to the changes in starch structure and morphology, the first component can reach a deeper penetration level alone or together with the second component. This further increases the difficulty of the first component being lost, so that the first component in the chitosan-acrylamide composite phenolic resin adhesive of this embodiment is almost not lost.

[0033] The change in starch structure and morphology by the first component not only promotes the penetration of the first component, blocks the contact between mold and starch, and changes the pH value of wood or bamboo fibers, but also: (1) the change in starch structure and morphology promotes the penetration of the second component, allowing the phenolic resin adhesive to penetrate not only into the gaps between wood or bamboo fibers, but also into the cells of wood or bamboo fibers, forming a complete and continuous adhesive penetration layer, thereby improving the internal bonding strength of the reconstructed or composite materials prepared using the composite phenolic resin adhesive; (2) the weakly alkaline pH value makes the wood or bamboo fiber environment more conducive to the curing of the thermosetting phenolic resin adhesive, thereby improving the internal bonding strength of the reconstructed or composite materials prepared using the composite phenolic resin adhesive.

[0034] In summary, the chitosan-acrylamide composite phenolic resin adhesive of this embodiment has a broad-spectrum and long-lasting mildew-proof performance. At the same time, the prepared recombinant or composite material has improved internal bonding strength.

[0035] As a preferred embodiment, the chitosan metal complex solution used is a chitosan-copper solution, and its concentration is 2%-3%. The preparation method of the chitosan-copper solution can be any one of the prior art, for example, 1g of solid chitosan is added to 100ml of a 0.1mol / L copper chloride solution, stirred for 8h under a pH value of 3.5, and then dechlorinated and vacuum dried to obtain solid chitosan-copper, which is dissolved in a 0.3% (v / v) hydrochloric acid solution to obtain 2%-3% chitosan-copper.

[0036] As a preferred embodiment, a chitosan-copper solution with a concentration of 2%-3% and an acrylamide solution with a concentration of 2%-3% are mixed in a ratio of 1:(0.5-2) to obtain a first component. The mixing method can be any one of the prior art, for example, stirring.

[0037] Taking into account the fungus inhibition effect and the water solubility of the first component, the preferred ratio of chitosan-copper solution to acrylamide solution is 1:1.

[0038] The first component and the second component can be applied to the treatment material (including but not limited to wood fiber, bamboo fiber, wood shavings, bamboo shavings, etc.) in sequence, or can be mixed and applied to the treatment material at the same time. When the first component and the second component are applied to the treatment material in sequence, if 1 part of the first component is used in the first step, 1 to 2.5 parts of the second component should be used in the second step; when the first component and the second component are pre-mixed and then applied to the treatment material, the first component and the second component are mixed in a ratio of 1: (1-2.5).

[0039] In one embodiment, the first component and the second component are applied to the treatment material one after the other, comprising the steps of: Step 1: immerse the material in the first component, first perform vacuum impregnation treatment (vacuum degree is -0.06MPa, treatment time is 50min), then perform pressure impregnation treatment (pressure is 1.5MPa, treatment time is 60min), and finally perform drying treatment (drying temperature is 45°C) to obtain the mildew-proof material; Step 2: immerse the anti-mildew material in the second component, first perform vacuum impregnation treatment (vacuuming for 15 minutes), and then perform drying treatment (drying to a moisture content of 8%-12%) to obtain the dipped anti-mildew material.

[0040] In another embodiment, the first component and the second component are pre-mixed and then used to treat the material. Specifically, the first component and the second component are mixed in proportion to obtain a composite phenolic resin adhesive, and the material is immersed in the second component to obtain the composite phenolic resin adhesive. First, a vacuum impregnation treatment is performed (the vacuum degree is -0.06MPa, and the treatment time is 50min), and then a pressurized impregnation treatment is performed (the pressure is 1.5MPa, and the treatment time is 60min). Finally, a drying treatment is performed (drying temperature 45°C, drying to a moisture content of 8%-12%) to obtain an impregnated mildew-proof material.

[0041] Regardless of the implementation method, the obtained impregnated mildew-proof material is assembled and then pressed at 125° C. for 10 minutes to obtain a recombinant or composite material.

[0042] The prepared recombinant or composite material is tested for mildew resistance, agent loss rate, static bending strength, and internal bonding strength.

[0043] Embodiment 1: This embodiment provides a chitosan-acrylamide composite phenolic resin adhesive, comprising a first component and a second component. The first component comprises a chitosan-copper solution with a concentration of 2% and an acrylamide solution with a concentration of 2%, and the chitosan-copper solution and the acrylamide solution are added in a ratio of 1:0.5. The second component comprises an aqueous, thermosetting phenolic resin adhesive with a solid content of 30%.

[0044] The first component and the second component are applied to the treated material in sequence, and the ratio of the first component to the second component is 1:1. The material is bamboo fiber, which is compressed to obtain a density of 1.23g / cm 3 of reconstructed bamboo.

[0045] Embodiment 2: This embodiment provides a chitosan-acrylamide composite phenolic resin adhesive, comprising a first component and a second component. The first component comprises a chitosan-copper solution with a concentration of 2% and an acrylamide solution with a concentration of 2%, and the chitosan-copper solution and the acrylamide solution are added in a ratio of 1:1. The second component comprises an aqueous, thermosetting phenolic resin adhesive with a solid content of 30%.

[0046] The first component and the second component are applied to the treated material in sequence, and the ratio of the first component to the second component is 1:1. The material is bamboo fiber, which is compressed to obtain a density of 1.23g / cm 3 of reconstructed bamboo.

[0047] Embodiment 3: This embodiment provides a chitosan-acrylamide composite phenolic resin adhesive, comprising a first component and a second component. The first component comprises a chitosan-copper solution with a concentration of 2% and an acrylamide solution with a concentration of 2%, and the chitosan-copper solution and the acrylamide solution are added in a ratio of 1:1. The second component comprises an aqueous, thermosetting phenolic resin adhesive with a solid content of 30%.

[0048] The first component and the second component are applied to the treated material in sequence, and the ratio of the first component to the second component is 1:2. The material is bamboo fiber, which is compressed to obtain a density of 1.23g / cm 3 of reconstructed bamboo.

[0049] Example 4: The embodiment provides a chitosan-acrylamide composite phenolic resin adhesive, comprising a first component and a second component. The first component comprises a chitosan-copper solution with a concentration of 3% and an acrylamide solution with a concentration of 3%, and the chitosan-copper solution and the acrylamide solution are added in a ratio of 1:2. The second component comprises an aqueous, thermosetting phenolic resin adhesive with a solid content of 30%.

[0050] The first component and the second component are applied to the treated material in sequence, and the ratio of the first component to the second component is 1:2.5. The material is bamboo fiber, which is compressed to obtain a density of 1.23g / cm 3 of reconstructed bamboo.

[0051] Embodiment 5: This embodiment provides a chitosan-acrylamide composite phenolic resin adhesive, comprising a first component and a second component. The first component comprises a chitosan-copper solution with a concentration of 2% and an acrylamide solution with a concentration of 2%, and the chitosan-copper solution and the acrylamide solution are added in a ratio of 1:1. The second component comprises an aqueous, thermosetting phenolic resin adhesive with a solid content of 30%.

[0052] The first component and the second component are added in a ratio of 1:1, and after mixing, a composite phenolic resin adhesive is obtained, and the composite phenolic resin adhesive is applied to the treatment material. The material is bamboo fiber, and the density is 1.23g / cm obtained by pressing. 3 of reconstructed bamboo.

[0053] Embodiment 6: This embodiment provides a chitosan-acrylamide composite phenolic resin adhesive, comprising a first component and a second component. The first component comprises a chitosan-copper solution with a concentration of 2% and an acrylamide solution with a concentration of 2%, and the chitosan-copper solution and the acrylamide solution are added in a ratio of 1:1. The second component comprises an aqueous, thermosetting phenolic resin adhesive with a solid content of 30%.

[0054] The first component and the second component are added in a ratio of 1:2, and after mixing, a composite phenolic resin adhesive is obtained, and the composite phenolic resin adhesive is applied to the treatment material. The material is bamboo fiber, which is pressed to obtain a density of 1.23g / cm 3 of reconstructed bamboo.

[0055] Embodiment 7: This embodiment provides a chitosan-acrylamide composite phenolic resin adhesive, comprising a first component and a second component. The first component comprises a chitosan-copper solution with a concentration of 2% and an acrylamide solution with a concentration of 2%, and the chitosan-copper solution and the acrylamide solution are added in a ratio of 1:1. The second component comprises an aqueous, thermosetting phenolic resin adhesive with a solid content of 30%.

[0056] The first component and the second component are added in a ratio of 1:2, and after mixing, a composite phenolic resin adhesive is obtained, and the composite phenolic resin adhesive is applied to the treated material. The material is wood shavings, and the density is 1.0g / cm 3 Wooden particle board.

[0057] Comparative Example 1: This comparative example uses a water-based, thermosetting phenolic resin adhesive with a solid content of 30%. The material is bamboo fiber, dried to a moisture content of 8%-12%, and the density is 1.23g / cm by pressing. 3 of reconstructed bamboo.

[0058] Comparative Example 2: This comparative example uses a water-based, thermosetting phenolic resin adhesive with a solid content of 30%. The material is carbonized bamboo fiber, dried to a moisture content of 8%-12%, and pressed to obtain a density of 1.23g / cm 3 of reconstructed bamboo.

[0059] Comparative Example 3: This comparative example uses a 2% chitosan-copper solution and a 30% solid content water-based, thermosetting phenolic resin adhesive, which are applied to the treated material in sequence, with the ratio of the first component to the second component being 1:1. The material is bamboo fiber, which is pressed to obtain a density of 1.23 g / cm 3 of reconstructed bamboo.

[0060] Comparative Example 4: This comparative example uses a water-based, thermosetting phenolic resin adhesive with a solid content of 30%. The material is wood shavings, dried to a moisture content of 8%-12%, and pressed to obtain a density of 1.0g / cm 3 Wooden particle board.

[0061] Comparative Example 5: This comparative example uses a 2% chitosan-copper solution and a 30% solid content water-based, thermosetting phenolic resin adhesive, which are applied to the treated material in sequence, with the ratio of the first component to the second component being 1:2. The material is wood shavings, which are pressed to obtain a density of 1.0 g / cm 3 Wooden particle board.

[0062] Figure 4 and Figure 5 The mildew resistance test results of the recombinant bamboo of Example 2, Example 5, and Comparative Examples 1-3 and the mildew resistance test results after the anti-loss experiment are shown respectively.

[0063] Table 1 shows the test results of the mildew resistance level of the recombinant or composite materials of Examples 1-7 and Control Examples 1-5, which are performed according to GB / T 18261-2013, with a cycle of 28 days, and the tested strains are Penicillium citrinum (PC), Aspergillius niger (AN) and Trichoderma viride (TV).

[0064] Table 2 shows the test results of the mildew resistance grade of the recombinant or composite materials of Examples 1-7 and Control Examples 1-5 after the anti-loss experiment. After the anti-loss experiment was performed according to GB / T 29905-2013, the mildew resistance grade after the anti-loss experiment was obtained according to GB / T 18261-2013. The cycle was 28 days, and the tested strains were Penicillium citrinum (PC), Aspergillius niger (AN) and Trichoderma viride (TV).

[0065] Table 3 shows the test results of the drug loss rate of Example 2 and Example 4, which were performed in accordance with GB / T 29905-2013.

[0066] Table 4 shows the test results of the static bending strength and internal bonding strength of the reconstructed or composite materials of Examples 1-7 and Comparative Examples 1-5. The static bending strength and internal bonding strength of the reconstructed bamboo are in accordance with GB / T 40247-2021, and the static bending strength and internal bonding strength of the wood particleboard are in accordance with GB / T 4897-2015.

[0067] Table 1 Table 2 Table 3 Group Drug loss rate / % Example 2 5.8 Example 5 2.9 Table 4 Group Static bending strength / MPa Internal bonding strength / MPa Example 1 41.3 0.65 Example 2 42.5 0.67 Example 3 41.7 0.64 Example 4 41.6 0.65 Example 5 43.9 0.69 Example 6 42.3 0.65 Example 7 14.9 0.55 Comparative Example 1 34.6 0.62 Comparative Example 2 32.4 0.57 Comparative Example 3 31.1 0.54 Comparative Example 4 14.2 0.48 Comparative Example 5 13.9 0.45 At least from Table 3 and Table 4, it can be known that even if the same components and proportions are used, compared with the technical solution of applying the first component and the second component to the material treatment in sequence, the technical solution of mixing the first component and the second component in advance to prepare the composite phenolic resin adhesive, and then applying the composite phenolic resin adhesive to the material treatment, has a lower drug loss rate. It is speculated that the reason for the above difference is that the former forms an impregnation layer in the bamboo fiber respectively, and the second component forms a solidified layer that covers the second component as a whole after solidification, and the latter is uniformly dispersed in the second component because the first component is uniformly dispersed in the second component, so as the second component solidifies, the second component wraps the liquid of the first component, which makes the second component lock the first component more stably, so Example 5 has a lower drug loss rate.

[0068] Due to the interaction between the first component and the second component, the static bending strength and internal bonding strength of the reconstructed or composite materials of Examples 1-7 are better.

[0069] The above description is intended to be illustrative and not limiting. Upon reading the above description, many embodiments and many applications beyond the examples provided will be apparent to those skilled in the art. Therefore, the scope of the present teachings should not be determined with reference to the above description, but should be determined with reference to the appended claims and the full scope of equivalents to which such claims are entitled. For the purpose of comprehensiveness, all articles and references, including disclosures of patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the preceding claims is not intended to be a waiver of the subject matter, nor should it be considered that the applicant has not considered the subject matter to be part of the disclosed application subject matter.

Claims

1. A chitosan-acrylamide composite phenolic resin adhesive, characterized in that: The invention comprises a first component and a second component, wherein the first component comprises a mixed chitosan metal complex solution and an acrylamide solution, and the second component comprises a phenolic resin adhesive.

2. The chitosan-acrylamide composite phenolic resin adhesive according to claim 1, characterized in that: The chitosan metal complex solution is a chitosan-copper solution.

3. The chitosan-acrylamide composite phenolic resin adhesive according to claim 1, characterized in that: The concentration of the chitosan metal complex solution is 2%-3%.

4. The chitosan-acrylamide composite phenolic resin adhesive according to claim 3, characterized in that: The addition ratio of the first component to the second component is 1:(1-2.5).

5. The chitosan-acrylamide composite phenolic resin adhesive according to claim 1, characterized in that: In the first component, the addition ratio of the chitosan metal complex solution to the acrylamide solution is 1:(0.5-2).

6. The chitosan-acrylamide composite phenolic resin adhesive according to claim 5, characterized in that: In the first component, the chitosan metal complex solution and the acrylamide solution are added in a ratio of 1:

1.

7. The chitosan-acrylamide composite phenolic resin adhesive according to claim 1, characterized in that: The first component is a graft copolymer solution of chitosan metal complex and acrylamide.

8. The chitosan-acrylamide composite phenolic resin adhesive according to claim 1, characterized in that: The first component and the second component are premixed.

9. An application of the chitosan-acrylamide composite phenolic resin adhesive as claimed in claim 1, characterized in that: At least the following steps are included: Step 1, immersing the material in the first component, first performing a vacuum impregnation treatment, then performing a pressure impregnation treatment, and finally performing a drying treatment to obtain a mildew-proof material; Step 2: immerse the anti-mildew material in the second component, first perform vacuum impregnation treatment, and then perform drying treatment to obtain the dipped anti-mildew material.

10. An application of the chitosan-acrylamide composite phenolic resin adhesive as claimed in claim 1, characterized in that: The first component and the second component are mixed in proportion to obtain a composite phenolic resin adhesive, the material is immersed in the second component to obtain the composite phenolic resin adhesive, firstly a vacuum impregnation treatment is performed, then a pressure impregnation treatment is performed, and finally a drying treatment is performed to obtain an impregnated mildew-proof material.

Citation Information

Cited By

  • Modified chitosan toughened phenol triazine resin and preparation method thereof

    CN121427103A