Phase change fiber, preparation method thereof and fiber fabric

By using the core-shell structure of polysiloxane or fluoropolymer and degradable polymer in the fiber, combined with electrospinning technology, the problems of low reflectivity and poor flexibility of radiation refrigerated fibers in the visible light range are solved, and the problem of low reflectivity and poor flexibility of radiation refrigerated fibers in the visible light range is achieved. Efficient radiation refrigeration performance and safe fiber preparation.

CN118996650APending Publication Date: 2024-11-22SHENZHEN UNIV
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411145416.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing radiation refrigerated fibers have low reflectivity in the visible range, poor daytime radiation effect, and the safety of nanomaterials have not been fully considered, and poor adhesion and softness of phase change materials.

Method used

Using a core-shell structure with polysiloxane or fluoropolymer as radiation reinforcement material and degradable polymer as shell material, and paraffin and other phase change materials as core material, phase change fibers are prepared through electrospinning technology, combined with superhydrophobic Self-cleaning surface design to improve fiber softness and radiation refrigeration performance.

Benefits of technology

It realizes efficient solar radiation reflection and mid-infrared radiation emission, maintains the softness of the fiber, enhances the radiation refrigeration performance, avoids the safety risks of nanomaterials, and improves the hydrophobicity and self-cleaning performance of the fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996650A_ABST
    Figure CN118996650A_ABST
Patent Text Reader

Abstract

The invention discloses a phase change fiber, a preparation method thereof and a fiber fabric, the phase change fiber has a core-shell structure with a radiation reinforcing material and a degradable polymer as shell materials and a phase change material as a core material, and the radiation reinforcing material is polysiloxane or a fluorine-containing polymer. The phase change material is packaged in the flexible polymer (the radiation enhancing material and the degradable polymer), so that leakage of the phase change material is prevented, the softness of the fabric is kept, and meanwhile, the problem that the refrigeration performance of the radiation refrigeration material is reduced due to environmental factors is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic materials, and in particular to a phase change fiber and a preparation method thereof and a fiber fabric. Background Art

[0002] As a clean, low-carbon and environmentally friendly passive cooling technology, radiative cooling can spontaneously dissipate heat and cool down without additional energy input, which can alleviate problems such as global warming. The temperature of the outer space (3K) outside the atmosphere is close to absolute zero, indicating that outer space contains a large amount of renewable thermal power resources and is an ideal radiative cooling source for the earth. In the wavelength range of 8-13μm, the atmosphere has high and medium infrared transmittance, so objects on the earth can radiate heat to outer space in the form of electromagnetic radiation. The ideal radiative cooling material needs to have high infrared radiation emissivity in the atmospheric window (8-13μm) and high solar radiation reflectivity in the wavelength range of 0.3-2.5μm of the solar spectrum. As a new type of refrigeration technology with zero energy consumption and zero pollution, radiative cooling plays an important role in energy-saving buildings, food storage, automobiles, smart wearables and electronic devices. Radiative cooling fabrics can be used in products such as outdoor tents, sun-proof clothing, car covers and shared bicycle seat covers, providing a new technical path for personal thermal management.

[0003] However, there are still limited examples of using radiation cooling for fabrics in existing public reports. Existing research mainly focuses on introducing particles with high mid-infrared emissivity on the surface of fabrics to improve the radiation characteristics of fabrics. Chinese invention patent CN110042564A discloses a radiation cooling fiber membrane, which prepares polymer fibers by electrospinning and dopes silica microspheres with high emissivity to achieve the purpose of radiation cooling. The fiber prepared by this method has high air permeability and can cool down by up to 2-7°C, but its reflectivity in the visible light range is low, and the daytime radiation effect is poor. It also requires a high-cost silver layer to achieve daytime radiation cooling. The selected inorganic functional particles such as titanium dioxide and silicon dioxide have weak selective solar reflection performance in the visible-near infrared spectral region, and it is difficult to obtain a more ideal cooling effect under lighting conditions. In addition, the safety of nanomaterials used in nanotechnology has not been pre-investigated. Nanomaterials are small in size and easy to enter human skin, which may have adverse effects on human cells. It has been proven that long-term, unprotected contact with nanoparticles can cause lung damage. Therefore, it is necessary to find more suitable and safer materials.

[0004] In addition, although radiative cooling materials have a certain cooling effect, the impact of the actual environment on the cooling effect of radiative cooling materials is not considered. When radiative cooling materials are exposed to outdoor environments, their surfaces will inevitably come into contact with rain and dust, which will increase solar energy absorption and reduce cooling efficiency. For the comfort of human body wearing, the design of super-hydrophobic self-cleaning surfaces becomes an important strategy. Furthermore, in the hot summer, the convective heat transfer generated by the hot air flow causes the temperature of the radiative cooling material to rise rapidly; on cloudy days, the transmittance of the atmospheric window is weakened, and the heat radiated by the radiative cooling material to outer space is reduced. At the same time, the existence of the heat accumulation effect will also cause the temperature of the radiative cooling material to gradually increase.

[0005] Phase change materials store and release thermal energy by responding to temperature, and have the advantages of large latent heat of phase change, no additional energy consumption, high energy storage density, constant temperature of storage and release, and recyclable. They are widely used in biomedicine, cold chain transportation, energy-saving buildings and other fields. The methods for acting phase change materials on fabrics generally include direct coating, cross-linking deposition, microencapsulation and composite spinning. Chinese invention patent CN115627643A proposes a super-hydrophobic fabric coating and a preparation method thereof. The patent adopts a spraying method to spray an aqueous polyurethane acrylate emulsion (containing hydrophobically modified silica / polyurea composite phase change microcapsules) on the surface of the fabric base fabric, and then bake it at 100°C for 3 minutes. However, this method has problems such as the attached phase change microcapsules are easily missed and migrated during use.

[0006] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0007] In view of the above-mentioned deficiencies in the prior art, the present invention provides a phase change fiber and a preparation method thereof and a fiber fabric, so as to solve the problems of poor adhesion of the existing phase change materials or phase change microcapsules and poor softness of the fiber fabric.

[0008] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0009] In a first aspect, the present invention provides a phase change fiber having a core-shell structure with a radiation enhancement material and a degradable polymer as shell materials and a phase change material as a core material, wherein the radiation enhancement material is polysiloxane or a fluorine-containing polymer.

[0010] Preferably, the polysiloxane is selected from one or more of polydimethylsiloxane, polycyclomethylsiloxane, polyaminosiloxane, and polymethylphenylsiloxane, and the fluorine-containing polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyvinylidene fluoride-hexafluoropropylene.

[0011] Preferably, the degradable polymer is one or more of polylactic acid, polyvinyl alcohol, polycaprolactone, polyadipate, polybutylene terephthalate, and cellulose acetate.

[0012] Preferably, the phase change material is selected from one or more of paraffin, n-octadecane, n-eicosane, n-heptadecane, polyethylene glycol, tetradecanol, methyl stearate, methyl palmitate, palmitic acid, and lauric acid.

[0013] The second aspect of the present invention further provides a method for preparing the above-mentioned phase change fiber, the preparation method comprising the following steps:

[0014] Dissolving the radiation enhancement material and the degradable polymer in a first organic solvent to obtain a shell material electrospinning solution;

[0015] dissolving the phase change material in a second organic solvent to obtain a core material electrospinning solution;

[0016] The shell material electrospinning solution is transferred to the first syringe and passed into the outer axis of the coaxial structure needle; the core material electrospinning solution is transferred to the second syringe and passed into the inner axis of the coaxial structure needle; and the phase change fiber is obtained by electrospinning.

[0017] Preferably, the conditions for the electrospinning are: the positive voltage of the spinning voltage is +10 to +20 kV, the negative voltage of the spinning voltage is -5 to -2 kV, the drum speed is 1000 to 2000 rpm, the distance between the syringe outlet end of the electrospinning equipment and the receiving substrate is 10 to 20 cm, the ambient temperature is 30 to 40 ° C, the ambient humidity is 30% to 45%, the pushing speed of the core material electrospinning solution is 0.05 to 0.5 mL / h, and the pushing speed of the shell material electrospinning solution is 1 to 3 mL / h.

[0018] Preferably, in the shell material electrospinning solution, the mass concentration of the radiation enhancement material is 5 to 15 wt%, and the mass concentration of the degradable polymer is 5 to 20 wt%;

[0019] In the core material electrospinning solution, the mass concentration of the phase change material is 50-100wt%.

[0020] Preferably, the first organic solvent and the second organic solvent are independently selected from one or two of dichloromethane, chloroform, toluene, xylene, N,N-dimethylformamide, and tetrahydrofuran;

[0021] The radiation enhancement material is polysiloxane or fluorine-containing polymer;

[0022] The polysiloxane is selected from one or more of polydimethylsiloxane, polycyclomethylsiloxane, polyaminosiloxane, and polymethylphenylsiloxane, and the fluorine-containing polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyvinylidene fluoride-hexafluoropropylene;

[0023] The degradable polymer is one of polylactic acid, polyvinyl alcohol, polycaprolactone, polyadipate, polybutylene terephthalate, and cellulose acetate;

[0024] The phase change material is selected from one or more of paraffin, n-octadecane, n-eicosane, n-heptadecane, polyethylene glycol, tetradecanol, methyl stearate, methyl palmitate, palmitic acid, and lauric acid.

[0025] According to a third aspect of the present invention, a fiber fabric is provided, wherein the fiber fabric is composed of the above-mentioned phase change fiber.

[0026] The fourth aspect of the present invention provides application of the above fiber fabric in the field of personal thermal management.

[0027] Beneficial effects:

[0028] In order to solve the influence of environmental factors on the cooling effect of the material, more phase change microcapsules are generally added to the fabric, which reduces the softness of the phase change fiber fabric to a certain extent. The present invention discloses a phase change fiber and its preparation method and fiber fabric, which encapsulates the phase change material in a flexible polymer (radiation enhancing material and degradable polymer), which is beneficial to prevent the leakage of the phase change material and maintain the softness of the phase change fiber fabric, and effectively solves the problem of reduced refrigeration performance of the radiation refrigeration material due to environmental factors. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of a fiber fabric provided in a preferred embodiment of the present invention;

[0030] Figure 2 This is a SEM image of the fiber fabric prepared in Comparative Example 1 of the present invention;

[0031] Figure 3 This is a SEM image of the fiber fabric prepared in Example 1 of the present invention;

[0032] Figure 4 TEM image of the fiber fabric prepared in Example 1 of the present invention

[0033] Figure 5 is the surface contact angle of the fiber fabric prepared in Comparative Example 1;

[0034] Figure 6 FTIR images of polydimethylsiloxane (PDMS), polylactic acid (PLA) and the fiber fabric (PLA / PDMS) prepared in Comparative Example 1;

[0035] Figure 7 DSC curves of polylactic acid (PLA), polydimethylsiloxane (PDMS), n-eicosane (C20) and the fiber fabric (PLA / PDMS@C20) prepared in Example 1;

[0036] Figure 8 The solar radiation reflection spectrum of the fiber fabric (PLA / PDMS) prepared in Comparative Example 1;

[0037] Fig. 9 The mid-infrared radiation emission spectrum of the fiber fabric (PLA / PDMS) prepared in Comparative Example 1;

[0038] Fig.10 Solar radiation reflection spectrum of the fiber fabric (PLA / PDMS@C20) prepared in Example 1;

[0039] Fig.11 The mid-infrared radiation emission spectrum of the fiber fabric (PLA / PDMS@C20) prepared in Example 1;

[0040] Fig.12 This is a physical picture of the fiber fabric prepared in Example 1. DETAILED DESCRIPTION

[0041] The present invention provides a phase change fiber and a preparation method thereof and a fiber fabric. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0042] The embodiment of the present invention provides a phase change fiber, wherein the phase change fiber has a core-shell structure with a radiation enhancement material and a degradable polymer as shell materials and a phase change material as core material, wherein the radiation enhancement material is polysiloxane or a fluorine-containing polymer, as shown in the schematic diagram Figure 1 shown.

[0043] The embodiment of the present invention encapsulates the phase change material in a flexible polymer (radiation enhanced material and degradable polymer), which is beneficial to preventing leakage of the phase change material and maintaining the softness of the phase change fiber, while effectively solving the problem of reduced refrigeration performance of the radiation refrigeration material due to environmental factors; further, the phase change material in the phase change fiber can store and release thermal energy by responding to temperature, thereby mitigating the impact of environmental factors on the refrigeration performance of the phase change fiber, which is beneficial to the application of the phase change fiber in complex environments.

[0044] In general, conventional atmospheric window radiation enhancement materials are mostly inorganic nanoparticles, such as silicon dioxide (SiO 2 ), titanium dioxide (TiO2 ) and aluminum oxide (Al 2 O 3 ), etc., while the use of inorganic nanoparticles mixed with polymer materials for electrostatic spinning will increase the viscosity of the spinning solution, resulting in an increase in the diameter of the generated fibers, and the weak solar reflection performance, making it difficult to obtain a more ideal cooling effect under lighting conditions. The embodiment of the present invention uses polysiloxane or fluorine-containing polymer as the atmospheric window radiation enhancement material, and composites it with a degradable polymer material to form a shell material, which improves the atmospheric window radiation emissivity while giving the fabric super-hydrophobic and self-cleaning properties.

[0045] Specifically, spectral control is particularly important for achieving high radiative cooling efficiency. In order to obtain the best cooling performance, the radiative cooling material is required to have a high solar radiation reflectivity in the 0.3-2.5μm wavelength range of the solar spectrum to limit the heat input of solar energy, and at the same time have a high infrared radiation emissivity in the atmospheric window (8-13μm) to effectively dissipate excess heat into the cold outer space. The infrared radiation generated by the degradable polymer in the atmospheric window actually originates from the vibration frequency generated by the chemical bonds and functional groups in the molecular structure of the degradable polymer. Different vibration frequencies have different absorption capabilities for the infrared spectrum. The functional group vibration fingerprint area (1500~600cm -1 The fingerprint region (7-16 μm) basically overlaps with the atmospheric window (8-13 μm), so degradable polymers with strong absorption functional groups in the fingerprint region can be used in radiation cooling materials. Since the bending vibration of functional groups such as CH, CO, C=O, Si-O-Si, and CF makes them have strong absorption in the fingerprint region, degradable polymers with these functional groups can have high-performance radiation cooling capabilities.

[0046] Therefore, the embodiment of the present invention selects polysiloxane or fluoropolymer (PDMS) as the atmospheric window radiation enhancement material, and composites it with a degradable polymer to form a composite shell material, which can improve the atmospheric window radiation emissivity (92.4%). At the same time, the surface of the radiation cooling material is inevitably in contact with rainwater and dust, which will lead to increased solar energy absorption and reduced cooling efficiency. The design of super-hydrophobic self-cleaning surface becomes an important strategy to ensure its optimal optical performance and radiation heat dissipation effect. Due to the low surface energy of polysiloxane or fluoropolymer (PDMS) and its weak adsorption capacity for water, the silicon-oxygen bonds in the PDMS molecules are arranged in a specific way to form a microstructure similar to the surface of a lotus leaf. This microstructure can reduce the actual contact area between water molecules and the surface of the radiation cooling material, thereby enhancing its hydrophobicity.

[0047] In addition, the embodiments of the present invention use degradable polymers, which have excellent performance and can be completely decomposed by environmental microorganisms after being discarded, and finally converted into CO 2 and H2 O and becomes an integral part of the carbon cycle in nature.

[0048] In some embodiments, the polysiloxane is selected from one or more of polydimethylsiloxane, polycyclomethicone, polyaminosiloxane, and polymethylphenylsiloxane, and the fluorine-containing polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyvinylidene fluoride-hexafluoropropylene. In some embodiments, the degradable polymer is one or more of polylactic acid, polyvinyl alcohol, polycaprolactone, polyadipic acid, polybutylene terephthalate, and cellulose acetate.

[0049] In some embodiments, the phase change material is selected from one or more of paraffin, n-octadecane, n-eicosane, n-heptadecane, polyethylene glycol, tetradecanol, methyl stearate, methyl palmitate, palmitic acid, and lauric acid.

[0050] The embodiment of the present invention provides a method for preparing the above phase change fiber, the preparation method comprising the following steps:

[0051] Dissolving the radiation enhancement material and the degradable polymer in a first organic solvent to obtain a shell material electrospinning solution;

[0052] dissolving the phase change material in a second organic solvent to obtain a core material electrospinning solution;

[0053] The shell material electrospinning solution is transferred to the first syringe and passed into the outer axis of the coaxial structure needle; the core material electrospinning solution is transferred to the second syringe and passed into the inner axis of the coaxial structure needle; and the phase change fiber is obtained by electrospinning.

[0054] In some embodiments, the electrospinning conditions are as follows: the positive voltage of the spinning voltage is +10 to +20 kV, the negative voltage of the spinning voltage is -5 to -2 kV, the drum speed is 1000 to 2000 rpm, the distance between the syringe outlet end of the electrospinning equipment and the receiving substrate is 10 to 20 cm, the ambient temperature is 30 to 40°C, the ambient humidity is 30% to 45%, the pushing speed of the core material electrospinning solution is 0.05 to 0.5 mL / h, and the pushing speed of the shell material electrospinning solution is 1 to 3 mL / h.

[0055] The control of electrospinning parameters is crucial to obtain the ideal phase change fiber diameter, morphological structure and to ensure the stability of the spinning process. Within this parameter range, a good phase change fiber morphology and distribution can be obtained, and stable jetting can also be ensured. Too high a voltage will cause the phase change fiber to have a beaded structure, uneven dispersion, bifurcation or breakage, and other undesirable phenomena; while too low a voltage will cause the phase change fiber to be blocked, unable to form a sufficient fiber network, and reduce production efficiency. The faster the receiving drum speed, the smaller the phase change fiber diameter, the worse the stability of the spinning process, and the dispersion and breakage rate of the phase change fiber will increase; the slower the speed, the larger the phase change fiber diameter, and problems such as fiber blocking or flutter are prone to occur. Too close a distance to the receiver will lead to uneven electrospinning; too far a distance will make the electrospinning too sparse or even impossible to spin. In addition, humidity and temperature will also affect the morphology of the phase change fiber. In an environment with low relative humidity, the electrospinning membrane is prone to charge accumulation and uneven distribution; while in a high humidity environment, fiber balls ("beads") and uneven dispersion are prone to occur. Too low or too high a temperature can easily lead to unstable droplets in the solution, which can interfere with the spinning process and affect the formation and morphology of the phase change fiber. The solution push speed within this parameter range can effectively improve the preparation efficiency and obtain uniform, smooth and complete cylindrical phase change fibers.

[0056] In some embodiments, in the shell material electrospinning solution, the mass concentration of the radiation enhancement material is 5 to 15 wt %, and the mass concentration of the degradable polymer is 5 to 20 wt %;

[0057] In the core material electrospinning solution, the mass concentration of the phase change material is 50-100wt%.

[0058] Within this parameter range, the stable formation and quality of spinning can be guaranteed, and the phase change fibers are smooth and have uniform diameters. If the concentration of the shell material electrospinning solution and the core material electrospinning solution is too low or the viscosity is insufficient, the jet may be unstable, thus affecting the formation and quality of the phase change fibers. When the solution concentration is too low, the molecular chains of the solution are not entangled enough, the force stretching is uneven, the molecular chain orientation coordination is inconsistent, and electrospraying will occur. Nano phase change fibers cannot be formed, but nano microspheres, i.e., "beaded" structure phase change fibers, will be formed; when the solution concentration is too high, the larger the diameter of the phase change fiber, the more aggregation will occur, affecting the formation of the phase change fiber.

[0059] In some embodiments, the first organic solvent and the second organic solvent are independently selected from one or two of dichloromethane, chloroform, toluene, xylene, N,N-dimethylformamide, and tetrahydrofuran;

[0060] The radiation enhancement material is polysiloxane or fluorine-containing polymer;

[0061] The polysiloxane is selected from one or more of polydimethylsiloxane, polycyclomethylsiloxane, polyaminosiloxane, and polymethylphenylsiloxane, and the fluorine-containing polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyvinylidene fluoride-hexafluoropropylene;

[0062] The degradable polymer is one of polylactic acid, polyvinyl alcohol, polycaprolactone, polyadipate, polybutylene terephthalate, and cellulose acetate;

[0063] The phase change material is selected from one or more of paraffin, n-octadecane, n-eicosane, n-heptadecane, polyethylene glycol, tetradecanol, methyl stearate, methyl palmitate, palmitic acid, and lauric acid.

[0064] An embodiment of the present invention provides a fiber fabric, wherein the fiber fabric is composed of the above-mentioned phase change fiber.

[0065] The fiber fabric provided by the embodiment of the present invention is formed by randomly stacking phase change fibers, and its porous structure enhances the diffuse reflection of solar radiation, so that the fiber fabric obtains a higher solar radiation reflectivity (such as 96.8%).

[0066] An embodiment of the present invention also provides an application of the above-mentioned fiber fabric in personal thermal management such as sun-protective clothing, car covers and shared bicycle seat covers.

[0067] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and are only for illustrating the present invention but not limiting the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0068] Example 1

[0069] A method for preparing a fiber fabric comprises the following steps:

[0070] (1) Preparation of shell material electrospinning solution: 4.23 g of dried polylactic acid particles (PLA) were mixed with a mixed solvent of N,N-dimethylformamide (DMF) and tetrahydrofuran (THF) in a volume ratio of 2:3 and added to a sealed conical flask (the concentration of polylactic acid was 12 wt%). The mixture was mechanically stirred for 2 h in a 50 °C water bath to obtain a polylactic acid solution. 0.846 g of polydimethylsiloxane (PDMS) and 0.08 g of DC184 curing agent (in a mass ratio of 10:1) were added to the polylactic acid solution and stirred for 12 h to fully mix the solution to obtain a shell material electrospinning solution.

[0071] (2) Preparation of core material electrospinning solution: 5 g of n-eicosane was dissolved in 3.33 g of chloroform and stirred for 2 h to obtain a core material electrospinning solution.

[0072] (3) Electrospinning: The shell material electrospinning solution and the core material electrospinning solution prepared above were transferred into a 10 mL syringe, and the syringe was connected to a coaxial spinning needle (24G / 16G, the inner and outer diameters of the inner needle were 0.27 mm and 0.55 mm, respectively, and the inner and outer diameters of the outer needle were 1.15 mm and 1.6 mm, respectively) through a catheter. The syringes were fixed on microinjection pumps, and the spinning needle was connected to the positive electrode of the high-voltage power supply, while the receiving roller was connected to the negative electrode; open Power supply, set the spinning process parameters: electrospinning voltage is positive voltage of +18kV, negative voltage is -2kV, receiving roller speed is 1000rpm, the distance from the receiving roller to the spinneret is 16cm, spinning temperature is 35℃, spinning humidity is 35%, core material electrospinning solution flow rate is 0.4mL / h, shell material electrospinning solution flow rate is 2mL / h for spinning, continuous spinning for 8h, and then put the spun product into a vacuum oven at 30℃ and dry it for 8h to obtain fiber fabric.

[0073] Example 2

[0074] A method for preparing a fiber fabric comprises the following steps:

[0075] (1) Preparation of shell material electrospinning solution: 4.23 g of dried polylactic acid particles (PLA) were mixed with a mixed solvent of N,N-dimethylformamide (DMF) and tetrahydrofuran (THF) in a volume ratio of 2:3 and added to a sealed conical flask (the concentration of polylactic acid was 12 wt%). The mixture was mechanically stirred for 2 h in a 50 °C water bath to obtain a polylactic acid solution. 0.846 g of polydimethylsiloxane (PDMS) and 0.08 g of DC184 curing agent (in a mass ratio of 10:1) were added to the polylactic acid solution and stirred for 12 h to fully mix the solution to obtain a shell material electrospinning solution.

[0076] (2) Preparation of core material electrospinning solution: 5 g of n-eicosane was dissolved in 2.5 g of chloroform and stirred for 2 h to obtain a core material electrospinning solution.

[0077] (3) Electrospinning: The shell material electrospinning solution and the core material electrospinning solution prepared above were transferred into a 10 mL syringe, and the syringe was connected to a coaxial spinning needle (24G / 17G, the inner and outer diameters of the inner needle were 0.27 mm and 0.55 mm, respectively, and the inner and outer diameters of the outer needle were 1.05 mm and 1.5 mm, respectively) through a catheter. The syringes were fixed on microinjection pumps, and the spinning needle was connected to the positive electrode of the high-voltage power supply, while the receiving roller was connected to the negative electrode; open Power supply, set the spinning process parameters: electrospinning voltage is positive voltage of +15kV, negative voltage is -2kV, receiving roller speed is 1000rpm, the distance from the receiving roller to the spinneret is 16cm, spinning temperature is 35℃, spinning humidity is 35%, core material electrospinning solution flow rate is 0.2mL / h, shell material electrospinning solution flow rate is 2mL / h for spinning, continuous spinning for 8h, and then the spun product is placed in a vacuum oven at 30℃ and dried for 8h to obtain fiber fabric.

[0078] Example 3

[0079] A method for preparing a fiber fabric comprises the following steps:

[0080] (1) Preparation of shell material electrospinning solution: 4 g of dried polylactic acid particles (PLA) were mixed with a mixed solvent of chloroform and N,N-dimethylformamide (DMF) in a volume ratio of 2:1 and added to a sealed conical flask (the concentration of polylactic acid was 10 wt%). The mixture was mechanically stirred for 2 h in a 50 °C water bath to obtain a polylactic acid solution. 0.846 g of polydimethylsiloxane (PDMS) and 0.08 g of DC184 curing agent (in a mass ratio of 10:1) were added to the polylactic acid solution and stirred for 12 h to fully mix the two to obtain a shell material electrospinning solution.

[0081] (2) Preparation of core material electrospinning solution: 5 g of n-octadecane was dissolved in 2 g of chloroform and stirred for 2 h to obtain a core material electrospinning solution.

[0082] (3) Electrospinning: The shell material electrospinning solution and the core material electrospinning solution prepared above were transferred into a 10 mL syringe, and the syringe was connected to a coaxial spinning needle (25G / 19G, the inner and outer diameters of the inner needle were 0.25 mm and 0.5 mm, respectively, and the inner and outer diameters of the outer needle were 0.72 mm and 1.02 mm, respectively) through a catheter. The syringes were fixed on microinjection pumps, and the spinning needle was connected to the positive electrode of the high-voltage power supply, while the receiving roller was connected to the negative electrode; open Power supply, set the spinning process parameters: electrospinning voltage is positive voltage of +15kV, negative voltage is -2kV, receiving roller speed is 1000rpm, the distance from the receiving roller to the spinneret is 18cm, spinning temperature is 40℃, spinning humidity is 40%, core material electrospinning solution flow rate is 0.2mL / h, shell material electrospinning solution flow rate is 2mL / h for spinning, continuous spinning for 8h, and then the spun product is placed in a vacuum oven at 30℃ and dried for 8h to obtain fiber fabric.

[0083] Comparative Example 1

[0084] A method for preparing a fiber fabric comprises the following steps:

[0085] (1) Preparation of spinning solution: 4.23 g of dried polylactic acid particles (PLA) and a mixed solvent of N,N-dimethylformamide (DMF) and tetrahydrofuran (THF) in a volume ratio of 2:3 were mixed and added to a sealed conical flask (the concentration of polylactic acid was 12 wt%). The mixture was mechanically stirred for 2 h in a 50°C water bath to obtain a polylactic acid solution. 0.846 g of polydimethylsiloxane (PDMS) and 0.08 g of DC184 curing agent (in a mass ratio of 10:1) were added to the polylactic acid solution and stirred for 12 h to fully mix the two to obtain a spinning solution.

[0086] (2) Electrospinning: The spinning solution prepared above was transferred into a 10 mL syringe, and the syringe was connected to a 16G spinning needle (with an inner diameter of 1.2 mm and an outer diameter of 1.64 mm) through a catheter. The syringe was fixed on a microinjection pump, and the spinning needle was connected to the positive electrode of a high-voltage power supply, while the receiving roller was connected to the negative electrode. The power was turned on, and the spinning process parameters were set as follows: the electrospinning voltage was +18 kV for the positive voltage and -2 kV for the negative voltage. The receiving roller speed was 1000 rpm, the distance from the receiving roller to the spinneret was 15 cm, the spinning temperature was 35°C, the spinning humidity was 35%, the spinning solution flow rate was 3 mL / h, and spinning was performed. The spinning was continued for 8 h, and then the spun product was placed in a vacuum oven at 30°C and dried for 8 h to obtain a fiber fabric.

[0087] The SEM image of the fiber fabric prepared in Comparative Example 1 is as follows: Figure 2 As shown in the figure, it can be seen that the phase change fiber is cylindrical in shape, with a smooth surface and uniform diameter distribution, and the diameter is about 650nm

[0088] The SEM image of the fiber fabric prepared in Example 1 is as follows: Figure 3 As shown in the figure, it can be seen that the surface of the phase change fiber maintains a complete cylindrical shape without any signs of damage, and the diameter is about 650nm; its TEM Figure 4 As shown, the phase change fiber has an obvious core-shell structure. The inner layer with darker color is the core layer of the phase change material, and the outer layer with lighter color is the polymer shell layer. The thickness of the shell layer is about 88nm, and the thickness of the core layer is about 475nm, proving that polydimethylsiloxane and polylactic acid successfully encapsulate the phase change material inside.

[0089] like Figure 5 As shown, the surface contact angle of the fiber fabric prepared in Comparative Example 1 is 153.96°, and the surface of the fiber fabric is super hydrophobic and has a self-cleaning effect.

[0090] Figure 6 The FTIR images of polydimethylsiloxane (PDMS), polylactic acid (PLA) and the fiber fabric (PLA / PDMS) prepared in Comparative Example 1 are shown. -1 The strong and broad absorption band at 795cm ​​is the symmetrical stretching vibration peak of Si-O-Si. -1 It is the symmetrical stretching vibration peak of Si-O bond; PLA is at 1750cm -1 There is a stretching vibration peak of C=O at 2975cm -1 The stretching vibration peak of the C-H bond is 1183 cm -1 and 1084cm -1 The stretching vibration peak of COC is at 795cm, and that of PLA / PDMS is at 795cm -1 There is a symmetrical stretching vibration peak of Si-O bond at 1081cm -1 The peak at represents the symmetric stretching vibration of Si-O-Si. The results show that PDMS exists in PLA / PDMS composite fibers.

[0091] Figure 7 The DSC curves of polylactic acid (PLA), polydimethylsiloxane (PDMS), n-eicosane (C20) and the fiber fabric (PLA / PDMS@C20) prepared in Example 1 are shown. The latent heat of phase change of n-eicosane is 242.83 J / g, and the latent heat of phase change of the fiber fabric prepared in Example 1 is 108.7 J / g; in addition, the crystallization and melting curves of polydimethylsiloxane and polylactic acid are both straight lines, proving that they do not undergo phase change behavior in the temperature range of 0-60°C, and at the same time indicating that the selection of polydimethylsiloxane and polylactic acid as packaging materials does not affect the latent heat of phase change of n-eicosane.

[0092] Figure 8The solar radiation reflectance spectrum of the fiber fabric (PLA / PDMS) prepared in Comparative Example 1 is shown, and the blue part in the figure is the solar radiation intensity distribution. Through calculation, its solar radiation reflectance is 95.6%.

[0093] Fig. 9 The figure shows the mid-infrared radiation emission spectrum of the fiber fabric (PLA / PDMS) prepared in Comparative Example 1. The blue part in the figure is the transmittance of the atmospheric window. Through calculation, its atmospheric window radiation emission rate is 91.4%.

[0094] Fig.10 The solar radiation reflectance spectrum of the fiber fabric (PLA / PDMS@C20) prepared in Example 1 is shown, and the blue part in the figure is the solar radiation intensity distribution. Through calculation, its solar radiation reflectance is 96.8%.

[0095] Fig.11 The figure shows the mid-infrared radiation emission spectrum of the fiber fabric (PLA / PDMS@C20) prepared in Example 1. The blue part in the figure is the transmittance of the atmospheric window. Through calculation, its atmospheric window radiation emissivity is 92.4%.

[0096] Fig.12 This is a physical picture of the fiber fabric prepared in Example 1.

[0097] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A phase change fiber, characterized in that: The phase change fiber has a core-shell structure with radiation enhancement material and degradable polymer as shell materials and phase change material as core material. The radiation enhancement material is polysiloxane or fluorine-containing polymer.

2. The phase change fiber according to claim 1, characterized in that: The polysiloxane is selected from one or more of polydimethylsiloxane, polycyclomethylsiloxane, polyaminosiloxane, and polymethylphenylsiloxane, and the fluorine-containing polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyvinylidene fluoride-hexafluoropropylene.

3. The phase change fiber according to claim 1, characterized in that: The degradable polymer is one or more of polylactic acid, polyvinyl alcohol, polycaprolactone, polyadipate, polybutylene terephthalate and cellulose acetate.

4. The phase change fiber according to claim 1, characterized in that: The phase change material is selected from one or more of paraffin, n-octadecane, n-eicosane, n-heptadecane, polyethylene glycol, tetradecanol, methyl stearate, methyl palmitate, palmitic acid, and lauric acid.

5. A method for preparing the phase change fiber according to claim 1, characterized in that: The preparation method comprises the following steps: Dissolving the radiation enhancement material and the degradable polymer in a first organic solvent to obtain a shell material electrospinning solution; dissolving the phase change material in a second organic solvent to obtain a core material electrospinning solution; The shell material electrospinning solution is transferred to the first syringe and passed into the outer axis of the coaxial structure needle; the core material electrospinning solution is transferred to the second syringe and passed into the inner axis of the coaxial structure needle; and the phase change fiber is obtained by electrospinning.

6. The method for preparing phase change fiber according to claim 5, characterized in that: The electrospinning conditions are as follows: the positive voltage of the spinning voltage is +10 to +20 kV, the negative voltage of the spinning voltage is -5 to -2 kV, the drum speed is 1000 to 2000 rpm, the distance between the syringe outlet end of the electrospinning equipment and the receiving substrate is 10 to 20 cm, the ambient temperature is 30 to 40 ° C, the ambient humidity is 30% to 45%, the pushing speed of the core material electrospinning solution is 0.05 to 0.5 mL / h, and the pushing speed of the shell material electrospinning solution is 1 to 3 mL / h.

7. The method for preparing phase change fiber according to claim 5, characterized in that: In the shell material electrospinning solution, the mass concentration of the radiation enhancement material is 5-15wt%, and the mass concentration of the degradable polymer is 5-20wt%; In the core material electrospinning solution, the mass concentration of the phase change material is 50-100wt%.

8. The method for preparing phase change fiber according to claim 5, characterized in that: The first organic solvent and the second organic solvent are independently selected from one or two of dichloromethane, chloroform, toluene, xylene, N,N-dimethylformamide, and tetrahydrofuran; The radiation enhancement material is polysiloxane or fluorine-containing polymer; The polysiloxane is selected from one or more of polydimethylsiloxane, polycyclomethylsiloxane, polyaminosiloxane, and polymethylphenylsiloxane, and the fluorine-containing polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyvinylidene fluoride-hexafluoropropylene; The degradable polymer is one of polylactic acid, polyvinyl alcohol, polycaprolactone, polyadipate, polybutylene terephthalate, and cellulose acetate; The phase change material is selected from one or more of paraffin, n-octadecane, n-eicosane, n-heptadecane, polyethylene glycol, tetradecanol, methyl stearate, methyl palmitate, palmitic acid, and lauric acid.

9. A fiber fabric, characterized in that: The fiber fabric is composed of the phase change fiber according to any one of claims 1 to 4.

10. Use of the fiber fabric according to claim 9 in the field of personal thermal management.

Citation Information

Cited By

  • Zero-energy-consumption double-module thermal management fabric and preparation method thereof

    CN119753923A

  • Phase-change temperature-control integrated negative electrode for energy storage lithium battery and preparation method of phase-change temperature-control integrated negative electrode

    CN120545313A

  • Bio-based thermal insulation coating composition, self-repairing bio-based thermal insulation coating and application thereof

    CN121227300A

  • Coaxial electrospinning radiation phase change cooling fiber membrane and preparation method thereof