Negative pole piece composite structure, preparation method thereof and lithium battery

By designing a rough surface and a mesh coating layer on the negative electrode sheet of the lithium-ion battery, cold pressing composite is achieved, and the problem of lithium-ion cell corner position is solved, and the composite rate and service life of the cell are improved.

CN119009377AActive Publication Date: 2024-11-22JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411107265.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

In the square winding process of lithium-ion batteries, the corner position of the battery cell causes wrinkles due to stress, resulting in excessive gap between positive and negative electrodes, insufficient electrolyte, resulting in lithium extraction, affecting the service life of the battery cell, and the existing technology composite The method has many steps, difficulty in ensuring uniformity, high energy consumption, and low recombination efficiency.

Method used

Adopt a composite structure of negative electrode sheets, including the electrode sheet body having a rough surface, the diaphragm is cold-pressed with the rough surface, and the glue coating layer is embedded on the rough surface. Through the design of slots and glue particles, it meets the specific ratio and distribution, and realizes the Cold pressing recombination avoids lithium evolution and improves the recombination rate.

Benefits of technology

The composite of the diaphragm and the pole sheet is completed without preheating, saving preheating time, avoiding lithium-ion separation at the corner of the battery cell, improving the composite rate, and improving the production efficiency and quality control of the battery cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009377A_ABST
    Figure CN119009377A_ABST
Patent Text Reader

Abstract

The invention discloses a negative pole piece composite structure, a preparation method thereof and a lithium battery, the negative pole piece composite structure comprises a pole piece body, one side of the pole piece body is provided with a rough surface; the diaphragm is arranged on one side, provided with the rough surface, of the pole piece body and is combined with the pole piece body in a cold pressing manner; and the gluing layer is arranged on the diaphragm and is embedded with a gap formed by the rough surface. According to the invention, through the arrangement, by utilizing the embedded acting force between the gluing layer and the pole piece body, the compounding of the diaphragm and the pole piece body can be completed under a cold pressing condition, namely, a preheating compounding mode in the prior art is not needed, so that the time required by preheating can be effectively saved, and the function of completing the compounding on the premise of not needing heating is achieved; and the aim of improving the compounding rate of the diaphragm and the pole piece to improve the productivity can be fulfilled while ensuring that lithium is not separated out at the corner of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a negative electrode plate composite structure, a preparation method thereof and a lithium battery. Background Art

[0002] Lithium-ion batteries (LIBs) have the advantages of high energy density, high operating voltage, long cycle life, low environmental pollution, low self-discharge, and no memory effect. They are considered to be one of the secondary batteries with the greatest development prospects. They are currently widely used in mobile phones, notebooks, cameras, portable tools, electric vehicles, energy storage, etc. With the rapid development of electric vehicles and energy storage, the demand for lithium-ion batteries is even more vigorous.

[0003] In the production process of square winding process batteries, in order to improve the wrinkling of the pole piece due to stress during the charging and discharging process, a single-sided or double-sided adhesive-coated diaphragm is often used to provide adhesion and stress release buffer. However, after the battery cell is wound, hot pressing can only be performed on the large surface, and the corners of the battery cell cannot be hot pressed. This leads to excessive gaps between the positive and negative poles of the pole piece at the corners in the middle and late stages of the cycle, coupled with insufficient electrolyte and bridge breakage, which ultimately leads to lithium deposition at the corners of the battery cell, thereby affecting the service life of the battery cell.

[0004] In the prior art, in order to avoid the service life of the battery cell being affected by lithium deposition at the corners of the battery cell, the following two technical means are usually used to achieve the above functions. Specifically, method 1: technical means such as glue coating at the corners are used to improve the liquid retention effect; method 2: the diaphragm and the negative electrode plate are thermally composited in advance, and then the composited plate and the positive electrode are wound.

[0005] However, both methods have certain defects: for example, method 1 requires more steps in actual operation, and it is difficult to ensure the uniformity of the glue coating, that is, it is difficult to ensure the quality control of the product; and method 2 requires the electrode or diaphragm to be preheated and then hot roller composited, which has high energy consumption and low composite efficiency, and is not conducive to increasing production capacity.

[0006] Therefore, a negative electrode plate composite structure, a preparation method thereof and a lithium battery are proposed to solve the above problems. Summary of the invention

[0007] The purpose of the present invention is to provide a negative electrode plate composite structure, a preparation method thereof and a lithium battery, so as to ensure that lithium is not deposited at the corners of the battery cell, while also improving the composite rate of the diaphragm and the plate, thereby achieving the purpose of increasing production capacity.

[0008] In order to solve the above technical problems, the present invention provides a negative electrode plate composite structure, comprising:

[0009] A pole piece body, one side of which has a rough surface;

[0010] A diaphragm, the diaphragm is arranged on the side of the pole piece body having the rough surface and is cold-pressed and combined with the pole piece body;

[0011] A rubber coating layer is disposed on the diaphragm and is embedded in the gap formed by the rough surface.

[0012] Furthermore, the rough surface includes a plurality of slots, and the rubber coating layer includes a plurality of rubber particles;

[0013] The negative electrode plate composite structure satisfies: 1.2≤L2 / L1≤2, 0.05≤H2 / H1≤0.2;

[0014] Wherein, L1 and H1 are respectively the maximum inner diameter and depth of the slot, and L2 and H2 are respectively the maximum outer diameter and thickness of the rubber particle.

[0015] Furthermore, the maximum inner diameter L1 of the slot is 50 μm-120 μm.

[0016] Furthermore, the depth H1 of the slot is one quarter to one half of the thickness of the pole piece body.

[0017] Furthermore, the distance D between two adjacent slots is 0.1 mm-4 mm.

[0018] Furthermore, the maximum outer diameter L2 of the colloid particles is 60 μm-240 μm.

[0019] Furthermore, the distribution number d of the colloidal particles is 4000 to 20000 / cm 2 .

[0020] Furthermore, the ratio of the maximum outer diameter L2 of the rubber particle to the maximum inner diameter L1 of the slot hole is 15:8, and the ratio of the thickness H2 of the rubber particle to the depth H2 of the slot hole is 1:10.

[0021] On the other hand, the present invention also provides a method for preparing a negative electrode plate composite structure, comprising the following steps:

[0022] Roughening the surface of the pole piece body to form a rough surface;

[0023] Applying a rubber coating layer on the diaphragm;

[0024] The adhesive coating layer and the rough surface are embedded under cold pressing conditions to complete the compounding of the pole piece body and the diaphragm.

[0025] Furthermore, the method for forming the rough surface includes laser etching and / or needle roller pressing.

[0026] Furthermore, the adhesive layer is coated on the diaphragm by spraying.

[0027] Furthermore, the embedding under cold pressing conditions includes adopting a double-roll cold pressing composite process.

[0028] On the other hand, the present invention further provides a lithium battery, comprising the negative electrode plate composite structure described in the above embodiment, or the negative electrode plate composite structure obtained by the preparation method described in the above embodiment.

[0029] Compared with the prior art, the present invention has at least the following beneficial effects:

[0030] By providing a pole piece body with a rough surface and providing a rubber layer on one side of the diaphragm that is embedded in the gap formed by the rough surface, the embedded force between the rubber layer and the pole piece body is utilized, so that the diaphragm and the pole piece body can be composited under cold pressing conditions, that is, there is no need to adopt the preheating composite method in the prior art, which can effectively save the time required for preheating and achieve the function of completing the composite without heating. In addition, due to the advance composite method of the diaphragm and the pole piece body, the service life of the battery cell can be effectively avoided due to lithium deposition at the corner of the battery cell. Therefore, while ensuring that lithium deposition will not occur at the corner of the battery cell, the composite rate of the diaphragm and the pole piece body can be improved to increase the production capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A schematic diagram of the structure of the negative electrode plate composite structure in one embodiment of the present invention

[0032] Figure 2 This is a flow chart of a method for preparing a negative electrode plate composite structure in another embodiment of the present invention.

[0033] Figure numbers: 1, pole piece body; 11, slot; 2, diaphragm; 3, rubber coating layer. DETAILED DESCRIPTION

[0034] The negative electrode plate composite structure of the present invention, its preparation method and lithium battery are described in more detail below in conjunction with schematic diagrams, wherein preferred embodiments of the present invention are shown, and it should be understood that those skilled in the art can modify the present invention described herein while still achieving the beneficial effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art and not as a limitation of the present invention.

[0035] The present invention is described in more detail in the following paragraphs by way of example with reference to the accompanying drawings. The advantages and features of the present invention will become more apparent from the following description. It should be noted that the accompanying drawings are in very simplified form and are not in exact proportions, and are only used to facilitate and clearly assist in illustrating the purpose of the embodiments of the present invention.

[0036] Embodiment 1

[0037] like Figure 1 As shown, an embodiment of the present invention provides a negative electrode plate composite structure, including:

[0038] The pole piece body 1 has a rough surface on one side. By setting the rough surface, the diaphragm 2 can achieve initial bonding with the help of the interlocking force between the adhesive layer 3 and the rough surface, and then the two can be composited under cold pressing conditions in the subsequent composite process. Therefore, compared with the hot pressing composite method in the prior art, the time required for preheating can be saved, thereby achieving the purpose of increasing production capacity.

[0039] It should be noted that, in this embodiment, the pole piece body 1 refers to the cathode piece.

[0040] The diaphragm 2 is arranged on the side of the pole piece body 1 having the rough surface, and is combined with the pole piece body 1 by cold pressing.

[0041] The adhesive layer 3 is arranged on the diaphragm 2 and is embedded in the gap formed by the rough surface. The diaphragm 2 and the pole piece body 1 are positioned by the embedding force between the adhesive layer 3 and the rough surface, thereby ensuring the normal progress of subsequent cold pressing and compounding.

[0042] By providing a pole piece body 1 with a rough surface and providing a rubber layer 3 on one side of the diaphragm 2 that is embedded in the gap formed by the rough surface, the embedded force between the rubber layer 3 and the pole piece body 1 is utilized to complete the compounding of the diaphragm 2 and the pole piece body 1 under cold pressing conditions, that is, there is no need to adopt the preheating compounding method in the prior art, thereby effectively saving the time required for preheating, and achieving the function of completing the compounding without heating. In addition, since the diaphragm 2 and the pole piece body 1 are compounded in advance, it is possible to effectively avoid the situation in which the service life of the battery cell is affected by lithium deposition at the corner of the battery cell. Therefore, while ensuring that lithium deposition will not occur at the corner of the battery cell, the compounding rate of the diaphragm 2 and the pole piece body 1 can be improved to increase the production capacity.

[0043] In a further embodiment, the rough surface and the rubber coating layer 3 are further limited to enhance the composite effect of the diaphragm 2 and the electrode body 1, and correspondingly enhance the subsequent production quality of the battery cell made of the negative electrode plate composite structure, that is, to ensure that the battery cell will not deposit lithium and the electrode body 1 will not be wrinkled.

[0044] Specifically, the rough surface includes a plurality of slots 11, and the rubber coating layer 3 includes a plurality of rubber particles.

[0045] The negative electrode plate composite structure satisfies: 1.2≤L2 / L1≤2, 0.05≤H2 / H1≤0.2, wherein L1 and H1 are respectively the maximum inner diameter and depth of the slot 11, and L2 and H2 are respectively the maximum outer diameter and thickness of the colloid particles. By limiting the maximum inner diameter and depth of the slot 11 and the maximum outer diameter and thickness of the colloid particles, the air permeability of the diaphragm 2 of the negative electrode plate composite structure is within a predetermined threshold, thereby improving the quality of the battery cell subsequently made of the negative electrode plate composite structure.

[0046] It should be noted that the air permeability of the diaphragm 2 indicates the effect of the negative electrode plate composite structure on the porosity of the diaphragm 2 after preparation. The permeability of the diaphragm 2 is measured by the time required for a unit area sample to pass 100cc of gas, in units of s / 100cc. Among them, the air permeability of the diaphragm 2 is closely related to the quality of the battery cell. Specifically, when the air permeability of the diaphragm 2 exceeds the established threshold, it will affect the lithium ion transmission in the later charging and discharging process, and the small interlayer spacing will also cause a certain degree of lithium precipitation; and when the air permeability of the diaphragm 2 is less than the established threshold, the adhesion between the diaphragm 2 and the plate body 1 is small, and it cannot play a good role in improving the interface, so it will cause the thickness of the battery cell to exceed the standard, affecting the production quality.

[0047] Therefore, by limiting the size of the slots 11 and the rubber particles, when the diaphragm 2 and the electrode body 1 are compounded, the air permeability of the diaphragm 2 can be within a predetermined threshold, thereby achieving the purpose of improving the quality of the battery cell.

[0048] Wherein, the maximum inner diameter L1 of the slot 11 is 50 μm-120 μm.

[0049] It should also be noted that the cross section of the slot 11 is an inverted trapezoidal structure, which effectively increases the contact area between the slot 11 and the rubber particles, thereby correspondingly increasing the interlocking force between the two, thereby facilitating the subsequent cold pressing composite between the diaphragm 2 and the pole piece body 1.

[0050] In addition, the depth H1 of the slot 11 is one quarter to one half of the thickness of the pole piece body 1 .

[0051] In a further embodiment, the distance D between two adjacent slots 11 is 0.1 mm-4 mm.

[0052] In other embodiments, the maximum outer diameter L2 of the colloid particles is 60 μm-240 μm, and the distribution number d of the colloid particles is 4000-20000 / cm 2 .

[0053] It should be noted that the distribution number d of the particles is linearly related to the maximum outer diameter L2 of the particles. For example, when the maximum outer diameter L2 of the particles is 150 μm, the distribution number d of the particles is 8000 / cm2 , so I won’t go into details here.

[0054] The rubber particles can be made of materials such as acrylic acid, acrylic ester, polyvinylidene fluoride, and polytetrafluoroethylene.

[0055] In this embodiment, a specific example is also proposed to better ensure that lithium deposition does not occur in the battery cell and wrinkles do not appear on the electrode body 1 .

[0056] Specifically, the ratio of the maximum outer diameter L2 of the rubber particle to the maximum inner diameter L1 of the slot 11 is 15:8, and the ratio of the thickness H2 of the rubber particle to the depth H1 of the slot 11 is 1:10.

[0057] The maximum outer diameter L2 of the colloid particle is 50 μm, the maximum inner diameter L1 of the slot 11 is 80 μm, the depth H1 of the slot 11 is 20 μm, the thickness H2 of the colloid particle is 2 μm, the distance D between two adjacent slots 11 is 2 mm, and the distribution number d of the colloid particles is 8000 / cm 2 .

[0058] As an example, the preparation method of the battery cell includes the following steps:

[0059] Preparation of positive electrode sheets: LiFePO4, SP and PVDF are uniformly dispersed in NMP in a mass ratio of 96.5%:1.5%:2% to form a positive electrode slurry, which is then coated, dried, rolled, slit, die-cut and made into positive electrode sheets to be wound.

[0060] Negative electrode sheet preparation: artificial graphite, SP, CMC and SBR are evenly dispersed in deionized water in a mass ratio of 96%: 1.2%: 1%: 1.8% to form a negative electrode slurry, which is then coated, dried, rolled, striped, surface punched or grooved, die-cut and separator 2 cold pressed to form a negative electrode sheet composite structure. Wherein L1 = 80μm, H1 = 20μm, L2 = 150μm, H2 = 2μm, D = 2mm, d = 8000 pieces / cm 2 .

[0061] The composite structure of the positive electrode sheet and the negative electrode sheet to be wound is wound into a battery cell, and the finished battery cell is obtained through processes such as assembly, liquid injection and formation.

[0062] It should also be noted that the preparation process of the positive electrode sheet and the preparation process of the battery cell are both existing technologies, so they will not be elaborated here. The difference between the preparation process of the negative electrode sheet and the traditional preparation process is that the diaphragm 2 can be combined with the negative electrode sheet by cold pressing. The remaining steps are consistent with the preparation of traditional negative electrode sheets, so they will not be elaborated here.

[0063] In addition, the following comparative examples are listed to demonstrate the application of battery cells when colloid particles of different sizes and slots 11 of different sizes are combined.

[0064] Comparative Example 1: L2 is 80 μm, and the rest is consistent with the above example.

[0065] Comparative Example 2: L2 is 280 μm, and the rest is consistent with the above example.

[0066] Comparative Example 3: H2 is 0.4 μm, and the rest is consistent with the above example.

[0067] Comparative Example 4: H2 is 5 μm, and the rest is consistent with the above example.

[0068] The specific test data are shown in Table 1 below:

[0069] Table 1

[0070]

[0071] It can be clearly observed from Table 1 above that when different colloid particles are fitted with slots 11 of different sizes, the air permeability of the diaphragm 2 will be obviously affected, which in turn will correspondingly affect the quality of the finished battery cell. Therefore, this product limits the relative relationship between the size of the colloid particles and the slots 11 (i.e., 1.2≤L2 / L1≤2, 0.05≤H2 / H1≤0.2) so that the air permeability of the diaphragm 2 can be within a predetermined threshold value, thereby effectively avoiding lithium deposition in the finished battery cell and wrinkles in the electrode body 1, thereby achieving the goal of ensuring that lithium deposition does not occur at the corners of the battery cell while increasing the recombination rate of the diaphragm 2 and the electrode body 1 to increase production capacity.

[0072] Embodiment 2

[0073] like Figure 2 As shown, this embodiment further proposes a method for preparing a negative electrode plate composite structure based on the first embodiment, comprising the following steps:

[0074] The surface of the pole piece body 1 is roughened to form a rough surface;

[0075] Applying a rubber coating layer 3 on the diaphragm 2;

[0076] The adhesive coating layer 3 is embedded with the rough surface under cold pressing conditions to complete the compounding of the pole piece body 1 and the diaphragm 2 .

[0077] By taking advantage of the embedded force between the rough surface and the rubber coating layer 3, the diaphragm 2 and the electrode body 1 can be initially positioned, so that the subsequent composite process can be directly completed by cold pressing. Therefore, compared with the hot pressing composite method in the prior art, the time required for preheating the diaphragm 2 and the electrode body 1 can be effectively shortened. Moreover, since the diaphragm 2 and the electrode body 1 (i.e., the cathode sheet) are composited in advance, the service life of the battery cell due to lithium deposition at the corners of the battery cell can be effectively avoided. Therefore, while ensuring that lithium deposition does not occur at the corners of the battery cell, the composite rate of the diaphragm 2 and the electrode body 1 can be increased to increase production capacity.

[0078] Among them, the method for forming the rough surface includes laser etching and / or needle roller rolling, that is, only a groove hole 11 for engaging with the adhesive layer 3 is formed on the pole piece body 1, and the engaging force between the adhesive layer 3 and the groove hole 11 can be used to complete the positioning work of the diaphragm 2 and the pole piece body 1 before cold pressing and compounding, thereby solving the defects of long preparation time and high energy consumption caused by hot pressing and compounding in the prior art.

[0079] In addition, the embedding under cold pressing conditions includes adopting a double-roll cold pressing composite process.

[0080] Embodiment 3

[0081] This embodiment provides a lithium battery, including the negative electrode plate composite structure described in the first embodiment, or the negative electrode plate composite structure obtained by the preparation method described in the second embodiment.

[0082] By providing a lithium battery with a negative electrode plate composite structure, it is possible to increase the recombination rate of the diaphragm and the electrode body while ensuring that lithium is not deposited at the corners of the battery cell, thereby achieving the purpose of increasing production capacity.

[0083] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A negative electrode plate composite structure, characterized in that: include: A pole piece body, one side of which has a rough surface; A diaphragm, the diaphragm is arranged on the side of the pole piece body having the rough surface and is cold-pressed and combined with the pole piece body; A rubber coating layer is disposed on the diaphragm and is embedded in the gap formed by the rough surface.

2. The negative electrode plate composite structure according to claim 1, characterized in that: The rough surface includes a plurality of slots, and the rubber coating layer includes a plurality of rubber particles; The negative electrode plate composite structure satisfies: 1.2≤L2 / L1≤2, 0.05≤H2 / H1≤0.2; Wherein, L1 and H1 are respectively the maximum inner diameter and depth of the slot, and L2 and H2 are respectively the maximum outer diameter and thickness of the rubber particle.

3. The negative electrode plate composite structure according to claim 2, characterized in that: The maximum inner diameter L1 of the slot is 50 μm-120 μm.

4. The negative electrode plate composite structure according to claim 2, characterized in that: The depth H1 of the slot is one quarter to one half of the thickness of the pole piece body.

5. The negative electrode plate composite structure according to claim 2, characterized in that: The distance D between two adjacent slots is 0.1 mm to 4 mm.

6. The negative electrode plate composite structure according to claim 2, characterized in that: The maximum outer diameter L2 of the colloid particles is 60 μm-240 μm.

7. The negative electrode plate composite structure according to claim 2, characterized in that: The distribution number d of the colloidal particles is 4000 to 20000 / cm 2 .

8. The negative electrode plate composite structure according to claim 2, characterized in that: The ratio of the maximum outer diameter L2 of the rubber particle to the maximum inner diameter L1 of the slot hole is 15:8, and the ratio of the thickness H2 of the rubber particle to the depth H2 of the slot hole is 1:

10.

9. A method for preparing a negative electrode plate composite structure according to any one of claims 1 to 8, characterized in that: The steps include: Roughening the surface of the pole piece body to form a rough surface; Applying a rubber coating layer on the diaphragm; The adhesive coating layer and the rough surface are embedded under cold pressing conditions to complete the compounding of the pole piece body and the diaphragm.

10. The preparation method according to claim 9, characterized in that: The rough surface is formed by laser etching and / or needle roller pressing.

11. The preparation method according to claim 9, characterized in that: The adhesive coating layer is applied on the diaphragm in a spraying manner.

12. The preparation method according to claim 9, characterized in that: The cold pressing condition embedding includes adopting a double-roll cold pressing composite process.

13. A lithium battery, characterized in that: It comprises a negative electrode sheet composite structure as described in any one of claims 1 to 8, or a negative electrode sheet composite structure obtained by the preparation method as described in any one of claims 9 to 12.

Citation Information

Patent Citations

  • Anti-wrinkle winding type positive pole piece, preparation method thereof and winding core

    CN116259707A

  • Ultrathin battery diaphragm, preparation method thereof and lithium ion battery

    CN117497959A

  • Pole piece structure, battery cell and lithium battery

    CN221008982U

  • Secondary battery and electric device

    WO2024113988A1

  • Secondary battery and electronic apparatus

    WO2024159521A1