Linear low density polyethylene, polymerization thereof, and films thereof

By developing polyethylene copolymers with specific density and melt index, the problem of insufficient melt fracture and processability of LLDPE during the extrusion process is solved, efficient and stable film production is achieved and production costs are reduced.

CN119013321APending Publication Date: 2024-11-22EXXONMOBIL CHEMICAL PATENTS INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380030690.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing linear low-density polyethylene (LLDPE) is prone to melt rupture during the extrusion process, resulting in surface roughness and flow disturbances, and its processability and mechanical characteristics are insufficient, making it difficult to achieve efficient production in commercial production.

Method used

A polyethylene copolymer was developed that contains ethylene units and 1-8 wt% of C3-C8α-olefin comonomer with a density of 0.914-0.925 g/cm3, a melt index of 1-2.5 g/10 min and 2 The molecular weight distribution of -8 is used to control the polymerization reaction conditions to maintain a small amount of long-chain branching and relatively consistent polymer chain distribution, reducing the viscosity consistency and avoiding adhesion problems.

Benefits of technology

The production of polyethylene copolymers on a commercial scale is achieved, which reduces motor torque and melt pressure during the extrusion process, reduces melt rupture, improves the bubble stability and production efficiency of the film, and avoids the use of fluorinated additives. necessity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005061448060000091
    Figure BDA0005061448060000091
  • Figure BDA0005061448060000092
    Figure BDA0005061448060000092
  • Figure BDA0005061448060000101
    Figure BDA0005061448060000101
Patent Text Reader

Abstract

The present disclosure relates to polyethylene polymers, polymerization processes for making such polyethylene polymers, and films made from such polyethylene polymers. In some embodiments, the polyethylene copolymer comprises ethylene units; and from 1 wt% to 8 wt% of Cs-Cs alpha-olefin comonomer units. The polyethylene copolymer has a density of from 0.914 g / cm3 to 0.925 g / cm3 and a melt index (MI, determined according to ASTM D1238 at 190 DEG C and a load of 2.16 kg) of greater than 1 g / 10 min and less than or equal to 2.5 g / 10 min. The polyethylene copolymer has a composition distribution width index of 75% or more and a molecular weight distribution (Mw / Mn) of 2 to 8.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of U.S. Provisional Application No. 63 / 362,239, filed on March 31, 2022, entitled “LINEAR LOW DENSITY POLYETHYLENES, POLYMERIZATIONS THEREOF, AND FILMS THEREOF,” the entire contents of which are incorporated herein by reference. Technical Field

[0002] The present disclosure relates to polyethylene polymers, polymerization processes for making such polyethylene polymers, and films made from such polyethylene polymers. Background Art

[0003] Linear low density polyethylene (LLDPE) is a substantially linear polymer consisting of ethylene monomer units and alpha-olefin comonomer units. The typical comonomer units used are derived from 1-butene, 1-hexene or 1-octene. LLDPE can be distinguished from conventional low density polyethylene (LDPE) in several ways, including their different manufacturing processes. In addition, LLDPE has little or no detectable long chain branching (LCB) / 1,000 carbon atoms, while conventional LDPE contains long chain branching. Long chain branching provides reduced shrinkage and increased tensile stability during the extrusion process. In addition, relative to the molecular weight distribution (MWD) of LDPE, LLDPE has a narrower MWD. ​​Compared with LDPE, LLDPE also has different rheological and mechanical properties, such as tear properties.

[0004] LLDPE formed using metallocene catalysts is called "mLLDPE". In order to match the extrusion rate of LDPE, the extrusion of mLLDPE requires more motor power and higher extruder pressure. Typical mLLDPE also has lower melt strength, which, for example, adversely affects bubble stability during blown film extrusion, and mLLDPE is prone to melt fracture at commercial shear rates. Melt fracture is a flow disturbance that causes surface roughness and / or surface irregularities in the extruded resin (including severe distortion of the extrudate). Melt fracture occurs when the shear stress imparted to the resin exceeds the critical shear stress value of the resin or creates slip-stick flow conditions in the die. Melt fracture may be associated with high die shear rates (e.g., 1,000-60,000 s -1 ) and the shear stress of such mLLDPE used to form the film. The high shear rate is a result of the high line speeds (e.g., >600 m / min) used to achieve mLLDPE films.

[0005] For many polyolefin applications (including films and fibers), increased melt strength is a desirable attribute. Higher melt strength allows manufacturers to run blown film production lines at a faster rate to form mLLDPE films. In order to improve and compensate for the above-mentioned melt fracture in the extrusion process, fluorinated additives such as PFAS (perfluoroalkanes or polyfluoroalkanes) are typically mixed with mLLDPE. However, such fluorinated additives are increasingly subject to regulatory scrutiny.

[0006] Regardless of the above processing and rheological challenges, mLLDPE does exhibit superior physical properties compared to LDPE. In the past, different levels of LDPE have been blended with mLLDPE to increase melt strength, increase shear sensitivity (e.g., increase flow at commercial shear rates in an extruder), and reduce the tendency for melt fracture. However, such blends typically have poor mechanical properties compared to pure mLLDPE. In fact, improving mLLDPE processability without sacrificing physical properties is a challenge.

[0007] Comparing LLDPEs to each other, LLDPEs with higher melt indexes are better for processing, and the combination of higher melt index and lower density is particularly good for cast film applications. However, less long chain branching can lead to reduced film properties. In practice, it is a challenge to find an LLDPE that has a combination of density and melt index while still being commercially processable.

[0008] In addition to the processing challenges described above, the polymerizations to form mLLDPE present their own challenges. For example, polyethylene with a higher melt index and lower density is expected to have a sticky consistency so that when formed in a reactor, the polyethylene will stick to the walls and other parts of the reactor, causing reactor shutdown.

[0009] Some references that may be of interest in this regard include: U.S. Patent Nos. 6,255,426, 7,951,873, 9,718,896, and 10,029,226; and U.S. Patent Publication Nos. US2004 / 0121098, US20070260016, US2015 / 0232589, and US2020 / 0339715.

[0010] In general, there is a need for new LLDPEs that have a combination of desirable properties such as density, melt index properties, long chain branching while also providing commercially desirable polymerization and extrusion of the LLDPE. Summary of the invention

[0011] In some embodiments, the polyethylene copolymer comprises ethylene units; and 1 wt% to 8 wt% of C3-C8 α-olefin comonomer units. The polyethylene copolymer has a molecular weight of 0.914 g / cm 3 Up to 0.925g / cm 3 Density, melt index of 1g / 10min to 2.5g / 10min, 5.8-10 is described as T 75 -T 25 The composition distribution width of 100 Å (° C.), the molecular weight distribution of 2 to 8, and the melt index ratio (MIR, which is defined as the ratio of the high load melt index (HLMI) to the melt index (MI)) in the range of 25 to 35 are described.

[0012] In some embodiments, the polyethylene copolymer comprises ethylene units; and 1 wt% to 8 wt% of C3-C8 α-olefin comonomer units. The polyethylene copolymer has a molecular weight of 0.914 g / cm 3 Up to 0.925g / cm 3 The polyethylene copolymer has a density of greater than 1 g / 10 min and a melt index (MI, which is determined according to ASTM D1238 at 190° C. and 2.16 kg load) of less than or equal to 2.5 g / 10 min. The polyethylene copolymer has a composition distribution breadth index of 75% or more and a molecular weight distribution (M w / M n ).

[0013] In some embodiments, the cast film comprises a polyethylene copolymer. The polyethylene copolymer has a molecular weight of 0.915 g / cm 3 Up to 0.917g / cm 3 The density and melt index of 1.6 g / 10 min to 1.8 g / 10 min.

[0014] In some embodiments, the blown film comprises a polyethylene copolymer. The polyethylene copolymer has a molecular weight of 0.915 g / cm 3 Up to 0.922g / cm 3 The density and melt index of 1.5 g / 10 min to 2.3 g / 10 min.

[0015] In some embodiments, a method for modeling the stickiness temperature of a polyethylene copolymer is included, wherein the polyethylene copolymer is manufactured in the presence of at least one catalyst. The method includes measuring the stickiness temperature of the polyethylene copolymer at each of multiple concentrations of an induced condensing agent in a test device. The method includes measuring the density, melt index (MI) and high load melt index (HLMI) of the polyethylene copolymer. The method includes calculating the melt flow ratio by dividing the HLMI by the MI. The method includes calculating the equivalent partial pressure of the induced condensing agent by accounting for the partial pressure of the isomers accumulated in the reactor. The method includes determining an equation that relates the stickiness temperature to the equivalent partial pressure based at least in part on the density, MI and MFR of the polyethylene copolymer. The polyethylene copolymer comprises ethylene units and 1wt% to 8wt% of C3-C8 alpha-olefin comonomer units. The polyethylene copolymer has a molecular weight of 0.914 g / cm 3 Up to 0.925g / cm 3 Density, melt index of 1g / 10min to 2.5g / 10min, T of 5.8-10 75 -T 25 (° C.) exhibiting a composition distribution width exhibited by a molecular weight distribution of 2 to 8, and a melt index ratio (MIR, which is defined as HLMI / MI) in the range of 25 to 35. The method can include producing additional polyethylene copolymers (e.g., in a polymerization reactor, the polymerization occurring in the presence of a polymerization catalyst) using the modeled viscosity temperature (e.g., using an equation relating the viscosity temperature to the equivalent partial pressure).

[0016] In some embodiments, a method for controlling polymerization to remain in a non-sticking regime is provided. The method includes measuring parameters of the polymerization reaction, the parameters including the concentration of the induced condensing agent (ICA) in the reactor temperature and the polymerization reactor. The method includes calculating the equivalent partial pressure of the ICA. The method includes positioning the polymerization reaction in a two-dimensional space defined by the reactor temperature dimension and the equivalent partial pressure dimension. The method includes comparing the position in the two-dimensional space with the non-sticking regime, which is defined as the space between the upper temperature limit curve and the lower temperature limit curve. The method includes adjusting one or more parameters of the polymerization to keep the polymerization in the non-sticking regime. The method includes obtaining a polyethylene copolymer from the polymerization reactor. The polyethylene copolymer comprises ethylene units and 1wt% to 8wt% of C3-C8 alpha-olefin comonomer units. The polyethylene copolymer has a molecular weight of 0.914 g / cm 3 Up to 0.925g / cm 3A density of , a melt index of 1 g / 10 min to 2.5 g / 10 min, a composition distribution width index of 75% or more, a molecular weight distribution of 2 to 8, and a melt index ratio (HLMI / MI) in the range of 25 to 35. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to be able to understand in detail the mode of the above enumerated features of the present invention, the present invention briefly summarized above can be described in more detail by referring to some of the embodiments shown in the accompanying drawings. However, it should be noted that the accompanying drawings only show typical embodiments of the present invention and are therefore not to be considered as limiting its scope, because the present invention may allow other equally effective embodiments.

[0018] Figure 1 is a process flow diagram of a method for measuring viscosity temperature according to an embodiment.

[0019] Figure 2 is a process flow diagram of a method of operating a reactor within a non-stick regime according to an embodiment.

[0020] Figure 3 is a graph of melt index versus density for conventional resins and inventive resins, according to embodiments.

[0021] Figure 4A are gel permeation chromatography chromatograms of the inventive resin and comparative resin according to an embodiment.

[0022] Figure 4B is a graph showing density versus EEE triad content for inventive resins and comparative resins according to embodiments.

[0023] Figure 5 is a graph showing viscosity flow curves at 190° C. of the present invention resin and comparative resin according to an embodiment.

[0024] Figure 6 is a graph showing VGP (Van Gurp Palman) curves of the present invention resin and comparative resin according to an embodiment.

[0025] Figure 7 is a graph showing temperature rising elution fractionation (TREF) chromatograms of the present resin and comparative resin according to the embodiment.

[0026] Figure 8 is a graph showing the melt strength of the resin of the present invention according to the embodiment.

[0027] Fig. 9 is a graph showing motor load, melt pressure, and melt temperature for film formation using the present invention resin and comparative resin according to an embodiment.

[0028] Fig.10 is a graph showing motor load, melt pressure, and melt temperature for film formation using the present invention resin and comparative resin according to an embodiment. DETAILED DESCRIPTION

[0029] Various embodiments and forms of disclosed compounds, methods and products will now be described, including specific embodiments and definitions adopted herein. Although specific embodiments are given in the following detailed description, it will be appreciated by those skilled in the art that these embodiments are exemplary only, and the embodiments of the present disclosure may be practiced in other ways. Any reference to an embodiment may refer to one or more of the compounds, methods or products defined by the claims, but not necessarily all. The use of titles is for convenience only and does not limit the scope of the present disclosure.

[0030] The present disclosure relates to polyethylene polymers, polymerization processes for making such polyethylene polymers, and films made from such polyethylene polymers. The polyethylene polymers are copolymers that have a combination of low density, high melt index, retention of long chain branching, and relatively consistent comonomer incorporation across polymer chains of varying lengths, while also providing commercially desirable polymerization and extrusion of the polyethylene copolymers.

[0031] Compared to conventional LLDPE, the polyethylene copolymers of the present disclosure can maintain a small amount of long chain branching (also referred to as "LCB") in the copolymer, thereby providing reduced shrink-in and increased tensile stability. The polyethylene copolymers of the present disclosure can exhibit a lower zero shear viscosity, resulting in lower motor torque and lower melt pressure and melt temperature during extrusion, thereby providing an increased yield of the extruded polyethylene copolymer product. In addition, because the LCB is maintained, the favorable processing characteristics are also maintained. For example, an approximately 10% reduction in motor torque and an approximately 25% reduction in melt pressure can be observed during cast film manufacturing (e.g., Figure 8 This small amount of LCB can be evidenced, for example, by a high melt index ratio and / or specific rheological characteristics, such as data obtained from small angle oscillatory shear (SAOS) experiments (e.g., η 0.01 / η 100 The ratio, η 0.01 and η 100 The complex viscosities are recorded at shear rates of 0.01 and 100 rad / s, respectively.

[0032] In addition, it has been found that the polyethylene copolymers of the present disclosure can provide excellent shear thinning characteristics, wherein the extrudate has little or no melt fracture at high die shear rates. For example, a polyethylene copolymer having a small amount of LCB with an MI of 1.5 to 2.5 g / 10 min and about 0.914 to 0.925 g / cm3 The polyethylene copolymers of the present disclosure of the combination of density of 1.5 to 2.5 can provide blown films with excellent bubble stability (little or no melt fracture), which allows polymer processing aids (such as perfluoroalkanes or polyfluoroalkanes) to be only unnecessary in the blown films of the present disclosure. The polyethylene copolymers of the present disclosure (e.g., a small amount of LCB with an MI of 1.5 to 2.5 and a density of 0.914 to 0.925 g / cm 3 The combination of a density of 100% and 100% (combination of ... Fig. 9 ). definition

[0033] As used herein, "olefins" may alternatively be referred to as "alkenes", and are linear, branched or cyclic compounds of carbon and hydrogen having at least one double bond. For purposes of this specification and the appended claims, when a polymer or copolymer is referred to as "comprising" an olefin, the olefin present in such a polymer or copolymer is the polymerized form of the olefin. For example, when a copolymer is described as having an "ethylene" content of 35 wt% to 55 wt%, based on the weight of the copolymer, it is understood that the monomer units in the copolymer are derived from ethylene in the polymerization reaction, and the derived units are present at 35 wt% to 55 wt%.

[0034] As used herein, the terms "polyethylene polymer", "polyethylene", "ethylene polymer", "ethylene copolymer" and "ethylene-based polymer" mean a polymer or copolymer comprising at least 50 mol% ethylene units, or at least 70 mol% ethylene units, or at least 80 mol% ethylene units, or at least 90 mol% ethylene units, or at least 95 mol% ethylene units or 100 mol% ethylene units (in the case of a homopolymer).

[0035] As used herein, "polymer" may refer to homopolymers, copolymers, interpolymers, terpolymers, and the like. A "polymer" has two or more monomeric units that are the same or different. A "homopolymer" is a polymer having the same monomeric units. A "copolymer" is a polymer having two or more monomeric units that are different from each other. A "terpolymer" is a polymer having three monomeric units that are different from each other. The term "different" as used to refer to monomeric units indicates that the monomeric units differ from each other by at least one atom or are isomerically different. Accordingly, as used herein, the definition of copolymer includes terpolymers, and the like. Likewise, as used herein, the definition of polymer includes copolymers, and the like.

[0036] As used herein, a particle size of greater than 0.860 to less than 0.910 g / cm 3 Ethylene polymers with a density of 0.910 to 0.925 g / cm 3 Ethylene polymers of a density of 0.925 to 0.940 g / cm2 are referred to as "linear low density polyethylene" (LLDPE) when substantially linear (with little or no long chain branching) (as is typical for Ziegler-Nata or metallocene-catalyzed PE) or as branched low density polyethylene (LDPE) when significantly branched (with a high degree of long chain branching) (as is typically the case for free radical polymerized PE); 0.925 to 0.940 g / cm2 3 Known as "medium density polyethylene" (MDPE); and has a density greater than 0.940 g / cm 3 Ethylene polymers with a density of 1000 Nm are called "high density polyethylene" (HDPE). Density is determined according to ASTM D792. Specimens are prepared according to ASTM D4703-Appendix 1 Procedure C, then conditioned according to ASTM D618-Procedure A and then tested.

[0037] As used herein, and unless otherwise specified, the term "Cn" means a hydrocarbon having n carbon atoms per molecule, where n is a positive integer.

[0038] As used herein, and unless otherwise specified, the term "hydrocarbon" means a class of compounds containing hydrogen bonded to carbon, and encompasses (i) saturated hydrocarbon compounds, (ii) unsaturated hydrocarbon compounds, and (iii) mixtures of hydrocarbon compounds (saturated or unsaturated), including mixtures of hydrocarbon compounds having different values ​​of n.

[0039] As used herein, the term "film" refers to a continuous, flat (in some cases flexible) polymer structure having an average thickness ranging from 0.1, or 1, or 5, or 10, or 15, or 20 μm to 50, or 75, or 100, or 150, or 200, or 250, or 1000, or 2000 μm, or such a coating of similar thickness attached to a flexible, non-flexible or other solid structure. A "film" can be made of or contain a single layer or multiple layers. Each layer can be made of or contain a polyethylene copolymer of the present disclosure. For example, one or more layers of a "film" can include a mixture of the disclosed polyethylene copolymer and LDPE, another LLDPE, polypropylene or a plastomer.

[0040] As used herein, a composition or film "free of" a certain component refers to a composition / film that is substantially free of the component, or comprises the component in an amount of less than about 0.01 wt % based on the weight of the total composition.

[0041] As used herein, the term "polymerizable conditions" refers to conditions that favor the reaction of one or more olefin monomers to produce a polyolefin polymer when contacted with an activated olefin polymerization catalyst, and includes the skilled artisan's selection of temperature, pressure, reactant concentrations, optional solvents / diluents, reactant mixing / addition parameters, and other conditions within at least one polymerization reactor.

[0042] For the sake of brevity, only some ranges are clearly disclosed herein. However, the scope of any lower limit can be combined with any upper limit to list the scope that is not clearly listed, and the scope of any lower limit can be combined with any other lower limit to list the scope that is not clearly listed, in this way, the scope of any upper limit can be combined with any other upper limit to list the scope that is not clearly listed. In addition, "in a range or within a range" includes each point or single value (even if not clearly listed) between its endpoints, and includes the endpoints themselves. Therefore, each point or single value can be combined with any other point or single value or any other lower limit or upper limit as its own lower limit or upper limit, to list the scope that is not clearly listed.

[0043] The term "terminal olefin" refers to a olefin having a structure ((R 1 R 2 )-C=CH2, where R 1 and R 2 can be independently hydrogen or any hydrocarbon group, such as R 1 is hydrogen, and R 2 is an olefin having a terminal carbon-carbon double bond in an alkyl group. A "linear terminal olefin" is a terminal olefin as defined in this paragraph wherein R 1 is hydrogen, and R 2 is hydrogen or a linear alkyl group.

[0044] The term "vinyl" means an olefin having the formula: Wherein R is a hydrocarbon group, such as a saturated hydrocarbon group, such as an alkyl group.

[0045] The term "vinylidene" means an olefin having the formula: Where R 1 and R 2 Each is independently a hydrocarbon group, such as a saturated hydrocarbon group, such as an alkyl group.

[0046] The term "vinylene" or "1,2-disubstituted vinylene" means (i) an olefin having the formula: or (ii) an olefin having the formula: or (iii) a mixture of (i) and (ii) in any proportion, Where R 1 and R 2 Each is independently a hydrocarbon group, such as a saturated hydrocarbon group, such as an alkyl group.

[0047] The term "trisubstituted vinylidene" means an olefin having the formula: Where R 1 , R 2 and R 3 Each is independently a hydrocarbon group, such as a saturated hydrocarbon group, such as an alkyl group. Polyethylene copolymer

[0048] The present disclosure provides polyethylene copolymers having a combination of low density, high melt index, low amount of long chain branching, and relatively consistent comonomer incorporation (high composition distribution breadth index (CDBI)) across polymer chains of varying lengths. In addition, polyethylene copolymers and films thereof can be formed by commercially desirable polymerization and extrusion of the polyethylene copolymers.

[0049] Thus, the polyethylene copolymers of various embodiments herein may exhibit one or more of the following properties: Density between 0.914 and 0.925 g / cm 3 , such as 0.914, 0.915, 0.916, 0.917, 0.918, 0.919 or 0.92 g / cm 3 Any lower end to 0.925, 0.924, 0.923, 0.922, 0.921, 0.920 or 0.919 g / cm 3 The higher end of any of the above, such as 0.915 g / cm 3 Up to 0.920g / cm 3 , alternatively 0.918 g / cm 3 Up to 0.922g / cm 3 In the range of 0.916 to 0.921 g / cm, any combination of the lower end to any higher end is contemplated (provided that the higher end is greater than the lower end), for example, 0.916 to 0.921 g / cm 3 . Melt index (MI, also known as I2 or I 2.16, according to the 2.16 kg load used in the test) is greater than 1.0 g / 10 min (ASTM D1238, 190°C, 2.16 kg), such as in the range of any low end of 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4 or 2.5 g / 10 min to any high end of 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 4 or 5 g / 10 min, wherein the range of any low end to any high end is contemplated herein (provided that the high end is greater than the low end), such as 1 to 2.5 g / 10 min, or 1.5 to 2 g / 10 min, such as 1.7 g / 10 min, etc. · Comonomer distribution reflects the similar degree of comonomer incorporation on polymer chains of different lengths of the polyethylene copolymer, which is quantified in terms of the composition distribution breadth index (CDBI). For example, the polyethylene comonomers of various embodiments have a CDBI of 70% or greater, such as 75% or greater, such as 80% or greater, 85% or greater, or even 90% or greater. The CDBI is defined as the weight percentage of copolymer molecules having a comonomer content within 50% of the median total molar comonomer content (i.e., within the range of 0.5x median to 1.5x median), and it is mentioned in, for example, U.S. Patent 5,382,630. In general, copolymers with a broader distribution result in a lower CDBI, while a theoretical copolymer with exactly the same relative comonomer content across all different lengths of the polymer chain would have a CDBI of 100%. The CDBI of a copolymer is readily determined using techniques for isolating individual fractions of a copolymer sample. One such technique is to use temperature rising elution fractionation (TREF) to generate a solubility distribution curve, as described in WO 1993003093 (which in this regard also refers to Wild et al., J.Poly.Sci.,Poly.Phys.Ed.[Journal of Polymer Science, Polymer Physics Edition] , Vol. 20, p. 441 (1982) and U.S. Pat. No. 5,008,204). All three of the foregoing publications are incorporated herein by reference. Alternatively, a narrow comonomer distribution may be reflected in the T 75 -T 25 Value, where T 25 is the temperature at which 25% of the eluted polymer is obtained, and T 75 is the temperature at which 75% of the eluted polymer is obtained, both obtained in a TREF experiment as described in US2019 / 0119413 (especially in paragraphs

[0055] -

[0058] thereof, which description is incorporated herein by reference). The narrow distribution is reflected in T 75 -T 25A relatively small difference in values, the difference being less than 10°C, such as in the range of 4°C to 10°C, such as at the low end of any one of 4°C, 4.5°C, 5°C, 5.5°C or 6°C to the high end of any one of 10°C, 9.5°C, 9°C, 8.5°C, 8°C, 7.5°C, 7°C or 6.5°C, such as 5.8°C to 7°C, alternatively 7°C to 9°C, wherein any combination of the low end to any high end is envisioned (provided that the high end is greater than the low end).

[0050] Polyethylene copolymer can be the polymerization product of ethylene monomer and one or more olefin comonomers (such as alpha-olefin comonomer).Alpha-olefin comonomer can have 3 to 12 carbon atoms or 4 to 10 carbon atoms or 4 to 8 carbon atoms.Olefin comonomer can be selected from the group consisting of: propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 4-methylpent-1-ene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-hexadecene etc. and any combination thereof, such as 1-butene, 1-hexene and / or 1-octene.In some embodiments, polyene is used as comonomer. In some embodiments, the polyene is selected from the group consisting of 1,3-hexadiene, 1,4-hexadiene, cyclopentadiene, dicyclopentadiene, 4-vinylcyclohex-1-ene, methyloctadiene, 1-methyl-1,6-octadiene, 7-methyl-1,6-octadiene, 1,5-cyclooctadiene, norbornadiene, ethylidene norbornene, 5-vinylidene-2-norbornene, 5-vinyl-2-norbornene, and olefins formed in situ in the polymerization medium. In some embodiments, the comonomer is selected from the group consisting of isoprene, styrene, butadiene, isobutylene, chloroprene, acrylonitrile, and cycloolefins. In some embodiments, a combination of olefin comonomers is utilized. In some embodiments, the olefin comonomer is selected from the group consisting of 1-butene and 1-hexene. The olefin comonomer content of the polyethylene copolymer can range from a low of about 0.1, 5, 5.5, 6, 6.5, 7, 7.5, 8, or 8.5 wt% to a high of about 20, 15, 13, 12.5, 12, 11.5, 11, 10.5, 10, 9.5, or 9 wt%, based on the total weight of monomers in the polyethylene copolymer. The remainder of the polyethylene comonomer is made up of units derived from ethylene (e.g., a low of 80, 85, 88, 90, 91, 92, 92.5, 93, 93.5, or 94 wt% to a high of 90, 91, 92, 92.5, 93, 93.5, 94, 94.5, 95, 95.5, 96, 97, 99, or 99.9 wt%). Ranges from any of the foregoing lower ends to any of the foregoing higher ends (eg, 88 to 93 wt%, such as 90 to 92.0 wt% ethylene-derived units with the balance being olefin comonomer-derived content) are contemplated herein.

[0051] The polyethylene copolymer may also have a high load melt index (HLMI) (also referred to as I HLMI) ranging from a low of 40, 45, 50, or 55 g / 10 min to a high of 75, 70, 65, 60, or 55 g / 10 min. 21 or I 21.6 , according to the 21.6 kg load used in the test); wherein any range from the aforementioned lower end to any aforementioned higher end (e.g., 45 to 70 g / 10 min, such as 45 to 55 g / 10 min, alternatively 60 to 70 g / 10 min) is contemplated herein. The term "high load melt index" ("HLMI") is the number of grams extruded in 10 minutes under the action of a standard load (21.6 kg), and is an inverse measure of viscosity. As provided herein, HLMI (I 21 ) is determined according to ASTM D1238 (190°C / 21.6 kg) and is sometimes referred to as I 21 or I 21.6 .

[0052] The polyethylene copolymer can have a melt index ratio (MIR, which is defined as I ) in the range of any of 20, 25, 26, 27, 28, 29, 30 or 31 on the low end to any of 40, 35, 34, 33, 32, 31 or 30 on the high end. 21.6 / I 2.16 Ratio), wherein any range from the aforementioned low end to any aforementioned high end (e.g., 27 to 33, such as 28 to 32, or 29 to 31) is contemplated herein, and MIR is 1 21 / I2 ratio.

[0053] The polyethylene copolymer may also have a molecular weight distribution (MWD) of about 2 to about 8. The MWD may also range from a low of about 2, 2.5, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, or 4 to a high of about 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 5, 6, or 8, wherein ranges from any of the foregoing low ends to any of the foregoing high ends are contemplated with the proviso that the high end of the range is greater than the low end. The MWD is defined as the weight average molecular weight (Mw) divided by the number average molecular weight (Mn).

[0054] The weight average molecular weight (Mw) of the polyethylene copolymers of various embodiments can range from 70,000 to 95,000 g / mol, such as 75,000 to 90,000 g / mol, such as 75,000 to 85,000 g / mol, alternatively 80,000 to 90,000 g / mol, wherein ranges from any of the foregoing lower ends to any of the foregoing higher ends are contemplated.

[0055] The number average molecular weight (Mn) of the polyethylene copolymers of various embodiments can range from 20,000 to 40,000 g / mol, such as 20,000 to 30,000 g / mol, such as 20,000 to 25,000 g / mol, with ranges from any of the foregoing lower ends to any of the foregoing higher ends being contemplated.

[0056] The Z-average molecular weight (Mz) of the polyethylene copolymers of various embodiments can be in the range of 150,000 to 190,000 g / mol, such as 154,000 to 175,000 g / mol, or 160,000 to 185,000 g / mol, such as 170,000 to 180,000 g / mol, wherein ranges from any of the foregoing lower ends to any of the foregoing higher ends are contemplated (e.g., 150,000 to 175,000 g / mol or 154,000 to 180,000 g / mol).

[0057] The polyethylene copolymers of various embodiments may also exhibit a small (but non-zero) amount of long chain branching. As previously noted, this can be seen, for example, by SAOS viscosity data (particularly η 0.01 / η 100 ) and / or MIR. In addition, the LCB index (g' or alternatively g'vis) can be less than 1, such as in the range of 0.9 to 0.99 or 0.94 to 0.98, but still significantly higher than g' for heavy-LCB polyethylene (such as LDPE made using free radical polymerization). Another useful parameter for indicating the presence of LCB is Figure 6 In particular, polyethylene copolymers (even LLDPE) with some LCBs will exhibit an inflection point in their VGP curves, whereas LLDPEs without any LCBs (e.g., Figure 6 The XP8318 does not show this inflection point.

[0058] The distribution and component (moment) of molecular weight (Mw, Mn, Mw / Mn, etc.) and branching index (g'vis) are determined by using a high temperature gel permeation chromatography (Polymer Char GPC-IR) equipped with an infrared detector IR5 based on a multi-channel bandpass filter, a 18-angle Wyatt Dawn Heleos light scattering detector and a 4-capillary viscometer with a Wheatstone bridge (Wheatstone bridge) structure. Three Agilent PLgel 10-μm Mixed-B LS columns are used to provide polymer separation. Aldrich reagent grade 1,2,4-trichlorobenzene (TCB) with 300ppm antioxidant butylated hydroxytoluene (BHT) is used as mobile phase. The TCB mixture is filtered through a 0.1-μm Teflon filter and degassed with an online degasser before entering the GPC instrument. The nominal flow rate is 1.0ml / min, and the nominal injection volume is 200μL. The whole system including transfer line, column and viscometer detector is contained in an oven maintained at 145°C. The polymer sample is weighed and sealed in a standard vial with 80-μL flow marker (heptane) added thereto. After the vial is loaded in the autosampler, the polymer is automatically dissolved in the instrument with 8ml of TCB solvent added. The polymer is dissolved at 160°C under continuous shaking for about 2 hours. The concentration (c) at each point in the chromatogram is calculated by the IR5 broadband signal intensity (I) minus the baseline using the following equation: c=βI, where β is the mass constant. The mass recovery rate is calculated by the ratio of the integral area of ​​the concentration chromatography in the elution volume to the injection mass (which is equal to the predetermined concentration multiplied by the injection loop volume). Conventional molecular weight (IR MW) is determined by combining a universal calibration relationship with a column calibration (which is carried out with a series of monodisperse polystyrene (PS) standards ranging from 700 to 10Mg / mol). The MW under each elution volume is calculated using the following equation: The variables with the subscript "PS" represent polystyrene, while those without the subscript are the test samples. In this method, α PS =0.67 and K PS=0.000175, while α and K are for ethylene-hexene copolymers, as calculated by empirical equations (Sun, T. et al. Macromolecules [macromolecules] 2001, 34, 6812), where a = 0.695 and K = 0.000579 (1-0.75Wt), where Wt is the weight fraction of the hexane comonomer. It should be noted that the comonomer composition is determined by the ratio of the IR5 detector intensities corresponding to the CH2 and CH3 channels, which are calibrated with a series of PE and ethylene-hexene homopolymer / copolymer standards (whose nominal values ​​are predetermined by NMR or FTIR). Here, the concentration is expressed in g / cm 3 denoted by , molecular weight is expressed in g / mol, and intrinsic viscosity (hence K in the Mark-Houwink equation) is expressed in dL / g.

[0059] The LS molecular weight (M) at each point in the chromatogram was determined by analyzing the LS output using the Zimm model for static light scattering. Here, ΔR(θ) is the excess Rayleigh scattering intensity measured at the scattering angle θ, c is the polymer concentration determined by IR5 analysis, A2 is the second virial coefficient, P(θ) is the shape factor of the monodisperse random coil, and Ko is the optical constant of the system: Among them, N A is Avogadro's number, and (dn / dc) is the refractive index increment of the system. The refractive index of TCB at 145°C and λ=665nm is n=1.500. For purposes of this disclosure and the claims thereto, for ethylene-hexene copolymers, (dn / dc)=0.1048.

[0060] The specific viscosity is determined using a high temperature Polymer Char viscometer with four capillaries arranged in a Wheatstone bridge configuration and two pressure sensors. One sensor measures the total pressure drop across the detector, and the other sensor, positioned between the two sides of the bridge, measures the pressure difference. The specific viscosity η of the solution flowing through the viscometer is s The intrinsic viscosity [η] at each point in the chromatogram is calculated from their output. s / c is calculated where c is the concentration and is determined from the IR5 broadband channel output.

[0061] The branching index (g'vis) is calculated using the output of the GPC-IR5-LS-VIS method as follows. Average intrinsic viscosity [η] of the sample avg By the following calculation: where the summation is performed over the chromatographic fragment i between the integration limits. Branching index g' vis Defined as Among them, M v is the viscosity average molecular weight based on molecular weight determined by LS analysis, and K and α are for a reference linear polymer, and for purposes of this disclosure, α and K are the same as described above for linear polyethylene polymers.

[0062] In addition, the polyethylene copolymer can have the following complex shear viscosity (η*) at 0.01 rad / s and 190°C: in the range of 5,000 to 12,000 Pa s; or 5,000, 6,000, 7,000, 8,000, 9,000, 10,000 or 11,000 Pa·s at a low end to 12,000, 11,000, 10,000, 9,000, 8,000, 7,000 or 6,000 Pa·s at a high end, wherein any low end to any high end range is contemplated (e.g., 6,000 to 8,000 Pa·s).

[0063] The complex shear viscosity (η*) at 100 rad / s and 190°C can be in the range of 900 to 2000 Pa·s; such as from a low end of any of 900, 1,000, 1,100 or 1,200 Pa·s to a high end of any of 1,200, 1,300, 1,400, 1,500 or 2,000 Pa·s, wherein ranges from any of the foregoing low ends to any of the foregoing high ends are also contemplated (e.g., 1,100 to 1,300 Pa·s).

[0064] In some embodiments, the polyethylene copolymer has a shear thinning ratio (η* at 0.01 / 100) of less than 15, or in the range of 3 to 15, or 4 to 12, or 5 to 10, or 5.5 to 8.

[0065] Rheological data such as "complex shear viscosity (η*)" reported in Pascal seconds can be measured at 0.01 rad / s and 100 rad / s. Complex shear viscosity and other rheological measurements can be obtained from small angle oscillatory shear (SAOS) experiments. For example, complex shear viscosity can be measured in a dynamic mode under a nitrogen atmosphere using parallel plates (diameter = 25 mm) using a rotational rheometer (such as an Advanced RheometricsExpansion System (ARES-G2 model) or a Discovery hybrid rheometer (DHR-3 model)). The rheometer can be thermally stabilized at 190°C for at least 20 minutes before the compression molded specimen is inserted onto the parallel plates. In order to determine the viscoelastic behavior of the sample, a frequency sweep in the range of 0.01 to 628 rad / s can be performed at a temperature of 190°C under a constant strain that does not affect the measured viscoelastic properties. The scanning frequency is equally spaced on a logarithmic scale so that 5 frequencies are detected every ten. Depending on the molecular weight and temperature, a strain of 3% may be used, and the linearity of the response is verified. A stream of nitrogen is circulated through the oven to minimize chain extension or crosslinking during the experiment. The specimens may be compression molded at 190°C without stabilizers. A sinusoidal shear strain may be applied. The shear thinning slope (STS) may be measured using a plot of the logarithm (base ten) of the dynamic viscosity versus the logarithm (base ten) of the frequency. The slope is 100s -1 log(dynamic viscosity) at a frequency of 0.01s -1 The difference in log(dynamic viscosity) at the frequency of the complex shear viscosity (η*) divided by 4. The curve of complex shear viscosity (η*) versus frequency (ω) can be fitted using the Carreau-Yasuda model: η*-η ∞ =(η 0- η ∞ )*(1+(λω) a ) (n-1) / a .

[0066] The five parameters in this model are: η0, the zero shear viscosity; λ, the relaxation time; and n, the power law exponent; η ∞ , infinite rate viscosity; and a, conversion index. When the dynamic viscosity is independent of frequency, the zero shear viscosity is the value at the plateau in the Newtonian region of the flow curve at low frequencies. The relaxation time corresponds to the inverse of the frequency at which shear thinning begins. The power law exponent describes the degree of shear thinning, because the magnitude of the slope of the flow curve at high frequencies on the log(η*)-log(ω) graph approaches n-1. For Newtonian fluids, n=1, and the dynamic complex viscosity is independent of frequency.

[0067] In addition to dynamic viscosity and complex viscosity (each in Pascal seconds), various other parameters including storage modulus (Pa), loss modulus (Pa), complex modulus (Pa), tan (δ), and phase angle were collected at each frequency sweep in the SAOS experiment. Plotting the phase angle from rheological experiments against the complex shear modulus produces a van Gurp Palmen plot that can be used to extract some information about molecular features, such as linear versus long chain branching, type of long chain branching, polydispersity (Dealy, MJ, Larson, RG, "Structure and Rheology of Molten Polymers", Carl Hanser Verlag, Munich 182-183 (2006). It has also been shown that VGP plots can be used to reveal the presence of long chain branching in polyethylene. See Trinkle, S., Walter, P., Friedrich, C. "Van Gurp-Palmen plot II—Classification of long chain branched polymers by their topology", 41 Rheol. Acta 103-113 (2002).

[0068] The "shear thinning ratio", reported as a unitless number, is characterized by a decrease in complex viscosity with increasing shear rate. Herein, shear thinning may be determined as the ratio of the complex viscosity at a frequency of 0.01 rad / s to the complex viscosity at a frequency of 100 rad / s.

[0069] In addition, the balance of some of the advantageous properties of the polyethylene copolymers of the present disclosure can be represented by an overall property called the "Q parameter." The Q parameter is represented by Equation 1: Q parameter = 0.001*(MIR*η 0.01 / η 100 ) 2 *(T 75 -T 25 ) / MWD (Equation 1) Where MIR is the melt index ratio, η 0.01 is the complex shear viscosity (η*) at 0.01 rad / s and 190°C, η 100 is the complex shear viscosity (η*) at 100 rad / s and 190°C, T 75 -T 25 It is T 75 -T25 Value, where T 25 is the temperature at which 25% of the eluted polymer is obtained and T 75 is the temperature at which 75% of the eluted polymer is obtained (determined by TREF, as mentioned above), and MWD is the molecular weight distribution. In some embodiments, the polyethylene copolymers of the present disclosure have a Q parameter of 50 to 90, such as 60 to 80, such as 60 to 70, alternatively 70 to 80. In general, the Q-parameters show a dependence on the LCB (via about the 4th power of the MIR and the viscosity ratio) and the breadth of the comonomer distribution (via T 75 -T 25 and thus, the Q-parameters capture the uniqueness of the combination of these properties exhibited in the polyethylene copolymers of the present disclosure.

[0070] In addition or instead, the polyethylene copolymer has a disubstituted vinylidene content of about 0.01 to about 0.1 disubstituted vinylidene / 1000 carbon atoms, such as about 0.02 to about 0.06 disubstituted vinylidene / 1000 carbon atoms. In some embodiments, the polyethylene copolymer has a trisubstituted vinylidene content of about 0.08 to about 0.2 trisubstituted vinylidene / 1000 carbon atoms, such as about 0.1 to about 0.15 trisubstituted vinylidene / 1000 carbon atoms. In some embodiments, the polyethylene copolymer has a vinyl content of about 0.01 to about 0.05 vinyl / 1000 carbon atoms, such as about 0.02 to about 0.04 vinyl / 1000 carbon atoms. In some embodiments, the polyethylene copolymer has a vinyl content of about 0.01 to about 0.05 vinylidene / 1000 carbon atoms, such as about 0.02 to about 0.04 vinylidene / 1000 carbon atoms.

[0071] You can use a 600MHz or higher 1 The spectrometer of H frequency was collected at 120 °C in a 10 mm probe 1HNMR data. Data can be recorded using a maximum pulse width of 45 °, 5 seconds between pulses, and an average of 512 transient signals. The spectrum signal is integrated. The polyethylene copolymer sample can be dissolved in deuterated 1,1,2,2-tetrachloroethane-d2 at a concentration of 30 mg / ml before being inserted into the spectrometer magnet. Before data analysis, the spectrum can be referenced by setting the residual hydrogen-containing solvent resonance to 5.98 ppm. The disubstituted vinylidene can be measured as the number of vinylidenes / 1,000 carbon atoms using the resonance between 5.55-5.31 ppm. The trisubstituted vinylidene ("trisub") end group can be measured as the number of trisubstituted groups / 1,000 carbon atoms using the resonance between 5.3-5.11 ppm according to the difference with the vinyl group. The vinyl end group can be measured as the number of vinyl groups / 1,000 carbon atoms using the resonance between 5.10-4.95 and 5.3-4.85 ppm. Vinylidene end groups can be measured as the number of vinylidene groups / 1,000 carbon atoms using the resonance between 4.84-4.70 ppm.

[0072] As used herein, a "triad" is a three-mer repeat unit that sums and is normalized to 1: for example, AAA, AAB, BAA, BAB, ABA, BBA, ABB, BBB. A = CH2; B = C6. By 13 C-NMR triad analysis provides insight into the sequence distribution and blockiness of the material. In some embodiments, the polyethylene copolymer has 13 C NMR ( 13 % to 94 mol%, such as 89 mol% to 92 mol%, such as 89 mol% to 91 mol% [EEE] triad content as determined by C NMR). ("E" is ethylene.) In some embodiments, the polyethylene copolymer has a triad content as determined by 13 3 mol % to 8 mol %, such as 4 mol % to 7 mol %, such as 5.3 mol % to 7 mol % [HEE] triad content as determined by C NMR. ("H" is hexene and "E" is ethylene). In some embodiments, the polyethylene copolymer has a triad content as determined by 13 0.05 mol % to 0.5 mol %, such as 0.1 mol % to 0.3 mol % [HEH] triad content as determined by C NMR. In some embodiments, the polyethylene copolymer has a triad content as determined by 13 The [EHE] triad content is from 1 mol % to 5 mol %, such as from 2 mol % to 4 mol %, as determined by C NMR.

[0073] for 13C NMR, the sample can be dissolved in deuterated 1,1,2,2-tetrachloroethane-d2 (tce-d2) at a concentration of 67 mg / mL at 140°C. The spectrum can be recorded at 120°C using a Bruker NMR spectrometer of at least 600 MHz with a 10 mm cryoprobe. 90° pulses, 10 s delay, 512 transients and gated decoupling can be used to measure 13 C NMR. The polymer resonance peak is referenced to the polyethylene main peak at 29.98 ppm. Chemical shift assignments for ethylene-based copolymers are described by Randall in "A Review Of High Resolution Liquid Carbon Nuclear Magnetic Resonance Characterization of Ethylene-Based Polymers", Polymer Reviews, 29:2, 201-5 317 (1989). Copolymer content, mole and weight %, triad ordering, and diad calculations are also calculated and described in the method established by Randall in this article. Olefins from waste processing

[0074] Processing of waste (such as plastic waste) can lead to the production or recovery of olefins, or attribute the waste feedstock to olefins (including any α-olefins disclosed herein), which are used to manufacture the polymer compositions disclosed herein (e.g., polyethylene copolymers). Waste can include plastic waste obtained from any source, including but not limited to urban, industrial, commercial or consumer sources. Plastic waste can further be obtained from common sources or from mixed sources (including mixed plastic waste obtained from urban or regional sources) and / or from waste streams of PET, HDPE, LDPE, LLDPE, polypropylene and / or polystyrene. In addition, waste can include thermoplastic elastomers and thermosetting rubbers, such as from tires and other products made of natural rubber, polybutadiene, styrene-butadiene, butyl rubber and EPDM.

[0075] The waste being processed may also include, without limitation, any of a variety of used polymeric and non-polymeric articles. Some examples of many types of polymeric articles may include: films (including cast films, blown films, and other forms), sheets, fibers, woven and non-woven fabrics, furniture (e.g., garden furniture), sporting equipment, bottles, food and / or liquid storage containers, transparent and translucent articles, toys, tubing and pipes, sheets, packaging, bags, sacks, coatings, caps, closures, crates, pallets, cups, non-food containers, barrels, insulators, and / or medical devices. Additional examples include automotive, aviation, marine, and / or watercraft parts (e.g., bumpers, grilles, trim parts, fenders, instrument panels, etc.), wire and cable sheathing, agricultural films, geomembranes, playground equipment, and other such articles, whether blow molded, rotationally molded, injection molded, etc. Any of the foregoing may include a mixture of polymeric articles and non-polymeric articles (e.g., packaging or other articles may include inks, paperboard, paper, metal deposits, etc.). One of ordinary skill will appreciate that such polymeric articles may be made from any of a variety of polymeric and / or non-polymeric materials, and that the polymeric materials may vary widely (e.g., ethylene-based, propylene-based, butyl-based polymers, and / or any C2 to C 40 or even higher olefins, and further include polymers based on any one or more types of monomers (e.g., C2 to C 40 Common examples include ethylene, propylene, butene, pentene, hexene, heptene and octene; and polyolefinic (including cycloolefin) monomers such as ethylidene norbornene (ENB) and vinylidene norbornene (VNB) (including, for example, when such cycloolefins are used as comonomers, such as in the case of ethylene monomers).

[0076] The processing of waste (such as by pyrolysis of plastic waste) can directly produce or recycle olefins for making such polymer compositions, or via the attribution production or recovery of these olefins for the system as a feed according to third-party certification about circularity, such as by crediting, allocating, and / or offsetting or replacing other hydrocarbons in the mass or energy balance of the system. Polymers whose circularity has been certified by third-party certification can be referred to as certified circular. An example of such certification is the mass balance custody chain method proposed by International Sustainability and Carbon Certification.

[0077] Various methods may be employed to produce, recover, or attribute olefins for use in the polymers disclosed herein. For example, olefins may be obtained from or in conjunction with co-processing of waste (e.g., plastic waste) with other hydrocarbon feeds in cracking, coking, hydroprocessing, and / or pyrolysis processes. For example, olefins may be directly or indirectly obtained from a fluid catalytic cracking unit, delayed coking unit, fluid coking unit (including FLEXICOKING) unit, or a combination thereof, which receives such waste as a feed or co-feed. TM Units), hydroprocessing units (including hydrocracking and hydrotreating units) and / or steam cracking units (including gas or liquid steam cracking units). Alternatively, such units may receive pyrolysis products of the processing of such wastes (such as separated or combined recycled pyrolysis gas and / or recycled pyrolysis oil) as feed or co-feed. Olefins can be produced directly by such a process or can be obtained by further processing (such as separation, treatment and / or cracking) the effluent of such a process. For example, olefins can be obtained by processing recycled pyrolysis oil and / or recycled pyrolysis gas produced from the pyrolysis of plastic waste. As used herein, "recycled pyrolysis oil" refers to a material composition that is liquid when measured at 25°C and 1atm, and at least a portion of which is obtained from the pyrolysis of recycled waste (e.g., recycled plastic waste). As used herein, "recycled pyrolysis gas" refers to a material composition that is gaseous at 25°C and 1atm, and at least a portion of which is obtained from the pyrolysis of recycled waste. In addition, wastes (such as plastic waste) are used as a feedstock in fluid catalytic cracking units, delayed coking units, fluid coking units (including FLEXICOKING TM Co-processing of feeds or co-feeds in hydroprocessing units (including hydrocracking and hydrotreating units), and / or steam cracking units (including gas or liquid steam cracking units) can result in attribution of the waste to the olefins, polymers, or polymer compositions described herein as determined by accounting for, allocating, and / or offsetting or replacing other hydrocarbons in the mass or energy balance of the system, as determined based on third-party certification regarding circularity.

[0078] Thus, the processes according to various embodiments herein may further include obtaining olefins that have been produced or recovered from the processing of plastic waste or olefins attributed to the processing of plastic waste, for example for use in a polymerization process as described elsewhere herein; and the polymer compositions (e.g., polyethylene copolymers) of various embodiments described herein may contain olefins that have been produced or recovered from the processing of plastic waste or olefins attributed to the processing of plastic waste. For example, at least a portion of the olefin content (e.g., employed in the method as described herein and / or contained in the composition as described herein) may come from olefins produced or recovered directly from the processing of plastic waste. Similarly, the processing of plastic waste may be attributed to at least a portion of the olefins (e.g., employed in the method as described herein and / or contained in the composition as described herein). Blends and Additives

[0079] In some embodiments, the polyethylene copolymer can be formulated (e.g., blended) with one or more other polymer components. In some embodiments, those other polymer components are alpha-olefin polymers, such as polypropylene or polyethylene homopolymers and copolymer compositions. In some embodiments, those other polyethylene polymers are selected from the group consisting of linear low density polyethylene, high density polyethylene, medium density polyethylene, low density polyethylene, and other differentiated polyethylenes.

[0080] In some embodiments, the formulated blend may contain additives that are determined based on the final use of the formulated blend. In some embodiments, the additive is selected from the group consisting of fillers, antioxidants, phosphites, anti-cling additives, tackifiers, UV stabilizers, heat stabilizers, anti-caking agents, mold release agents, antistatic agents, pigments, colorants, dyes, waxes, silica, processing aids, neutralizers, lubricants, surfactants, and nucleating agents. In some embodiments, the additive is present in an amount of 0.1 ppm to 5.0 wt%.

[0081] The polyethylene copolymers of the present disclosure may optionally be blended with one or more processing aids to form polyethylene blends. Due to the improved properties of the polyethylene copolymers of the present disclosure, advantageously, such processing aids may be omitted even in blown films (e.g., films of some embodiments, and in particular blown films, may be free of or substantially free of polymer processing aids, and in particular polymer processing aids containing fluorine; wherein "substantially free" means free of any intentionally added components, but allows up to 100 ppm of such components as impurities). Aggregation methods

[0082] The polymerization process may include gas phase polymerization, and in particular fluidized bed gas phase polymerization. Gas phase polymerization may be carried out in any suitable reactor system (e.g., a stirred or paddle reactor system). For discussion of suitable gas phase fluidized bed polymerization systems well known in the art, see U.S. Patent Nos. 7,915,357, 8,129,484, 7,202,313, 6,833,417, 6,841,630, 6,989,344, 7,504,463, 7,563,851, and 8,101,691.

[0083] It has been found that the polyethylene copolymers of the present disclosure can be formed using non-stick polymerization at a commercial scale. Appropriate polymerization parameters for preventing sticking in a reactor used to form the polyethylene copolymers of the present disclosure can be used as described in more detail below and in U.S. Pat. No. 9,718,896 (which is incorporated herein by reference). 粘性 " method to determine.

[0084] In this type of polymerization process, the gas phase fluidized bed process is carried out by continuously passing a stream containing ethylene and olefin comonomers through a fluidized bed reactor at a speed sufficient to keep a bed of solid particles in a suspended state under reaction conditions and in the presence of a catalyst composition. The stream containing unreacted ethylene and olefin comonomers (which can be referred to as a "cycle gas" stream) is continuously taken out from the reactor, compressed, cooled, partially or completely condensed alternatively, and recycled back to the reactor. The polyethylene copolymer prepared is taken out from the reactor, and the ethylene and olefin comonomers replaced are added to the recycle stream. In some embodiments, a gas inert to the catalyst composition and reactants is present in the gas stream.

[0085] The circulating gas may include an induced condensing agent (ICA). ICA is one or more non-reactive alkanes that are condensable in the polymerization process to remove heat of reaction. In some embodiments, the non-reactive alkanes are selected from C1-C6 alkanes, such as one or more of propane, butane, isobutane, pentane, isopentane, hexane, and isomers thereof and derivatives thereof. In some cases, mixtures of two or more such ICAs may be particularly desirable (e.g., propane and pentane, propane and butane, butane and pentane, etc.).

[0086] Reactor pressure can be from 100psig (680kPag)-500psig (3448kPag), or in the range of 200psig (1379kPag)-400psig (2759kPag), or in the range of 250psig (1724kPag)-350psig (2414kPag). In some embodiments, the reactor is operated at a temperature in the range of 60°C to 120°C, 60°C to 115°C, 70°C to 110°C, 70°C to 95°C, or 80°C to 90°C. The ratio of hydrogen to ethylene can be 10 to 30ppm / mol%, such as 15 to 25ppm / mol%, such as 16 to 20ppm / mol%.

[0087] The mole % of ethylene can be 25.0-90.0 mole %, or 50.0-90.0 mole %, or 70.0-85.0 mole %, and the ethylene partial pressure is in the range of 75 psia (517 kPa)-300 psia (2069 kPa), or 100-275 psia (689-1894 kPa), or 150-265 psia (1034-1826 kPa), or 180-200 psia. The ethylene concentration in the reactor may also be in the range of 35-95 mol%, such as in the range of 35, 40, 45, 50 or 55 mol% on the low end to 70, 75, 80, 85, 90 or 95 mol% on the high end, and further wherein the ethylene mol% is measured based on the total molar amount of gas in the reactor (including, if present, ethylene and / or comonomer gas and one or more of inert gases such as nitrogen, isopentane or other ICAs, etc.); as with vol-ppm hydrogen, for convenience this measurement may be made in the recycle gas outlet rather than in the reactor itself. The comonomer concentration may be in the range of 0.2-1.0 mol%, such as in the range of 0.2, 0.3, 0.4 or 0.5 mol% on the low end to 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 1.0 mol% on the high end. catalyst

[0088] The catalyst used in the polymerization can be a metallocene catalyst. Especially, the metallocene catalyst can be selected from the catalyst described in Patent Cooperation Treaty Publication No. WO 1993008221, WO 1996008520, WO 1998044011 and WO 2007130277, and these patents are incorporated herein by reference for all purposes. For example, the catalyst can be a silicon dioxide-loaded metallocene catalyst prepared by a composition comprising dimethylsilylbis (tetrahydroindenyl) zirconium dichloride metallocene and methylaluminoxane cocatalyst. In some embodiments, the catalyst is dimethylsilylbis (tetrahydroindenyl) zirconium dichloride. Non-stick polymerization

[0089] Described herein are systems and methods for determining a non-stick operating regime ("safe" regime) for a polymerization reactor, and operating a polymerization reactor within the non-stick regime, particularly to obtain polyethylene copolymers according to the above description. As used herein, a non-stick operating regime indicates a regime in which resin sticking to components of the reactor is not a problem. These methods may include developing a model of the non-stick operating regime that can be integrated into a control system or used on a separate system to control reaction parameters; controlling polymerization using the model; and obtaining polyethylene copolymers according to the above description.

[0090] The parameters used in the model for developing a non-stick operating scheme can be based on the values ​​measured during the experimental determination of resin viscosity. For a single target resin, resin viscosity can be measured as a function of temperature and the equivalent partial pressure of an induced condensing agent (referred to as "ICA"). For example, the measurement can be performed by placing the resin in a stirred autoclave reactor with a measured amount of ICA (such as isopentane (IC5)) and slowly raising the temperature until the resin becomes sticky, thereby causing the agitator to stall. A model that predicts the viscosity temperature as a function of the equivalent partial pressure of the reactor temperature and the ICA can then be constructed. Use the equivalent partial pressure to account for other condensable materials that may be present in the reactor, such as various isomers of hexene and hexene. The model is usually specific to the type of resin used.

[0091] The non-stick operating regime is determined using a model of the ICA used in the polymerization reaction and the dew point. During the polymerization reaction, the reactor is controlled to maintain the temperature and ICA concentration within the non-stick operating regime. By controlling the reaction parameters to allow both the temperature and ICA content to be increased, thereby allowing more heat of reaction to be removed, the non-stick operating regime can provide guidance to help maximize production rates without agglomeration.

[0092] As used herein, the term "diluent" (or "condensable diluent" or "condensable diluent gas") refers to a condensable gas (or mixture of condensable gases) present in a polymerization reactor producing a polymer resin. The diluent is condensable at the temperatures encountered in the process heat exchangers. Examples of diluents include induced condensing agents (ICAs), comonomers, isomers of comonomers, and combinations thereof. Such materials may include isobutane, isopentane, hexene, and other materials in the reactor.

[0093] Sample resins may be tested for stickiness in a test apparatus such as that described in US9,718,896 to gain a better understanding of the operability window for producing resins with various metallocene catalysts. Through testing on multiple catalysts, it can be determined that unique parameters may be developed for each of the multiple resins made using different catalysts. The stickiness risk associated with resins made with these catalysts may be reduced by using a combination of temperature, MI / density / MFR targets, ethylene partial pressure, induced condensing agent (e.g., IC5 or isohexane) concentration, and continuity additives.

[0094] A test device can be used to measure the viscosity temperature. The device can use an autoclave reactor with a mixing motor. The mixing motor rotates a mixer blade inserted into the resin bed in the autoclave. The temperature in the autoclave is slowly increased until the torque required to rotate the mixer blade overcomes the torque available from the mixing motor and the mixer blade stops rotating, indicating the temperature at which the resin is sticky or agglomerated. An exemplary mixing motor that can be used is an air-driven motor model #2AM-NCC-16 manufactured by Gast Manufacturing, Inc. The mixing motor rotates a magnetic coupler, which in turn causes the mixer blade to spin. An exemplary magnetic coupler that can be used is manufactured by Autoclave Engineers. 2.

[0095] The test apparatus can run viscosity experiments under dry conditions and also in the presence of induced condensing agents such as isopentane (IC5) and isohexane (IC6). Although details of a specific test apparatus are presented, it should be understood that any device capable of consistently measuring the torque of a rotating mixer blade can be used to develop a model for a specific resin.

[0096] Figure 11 is a process flow chart showing a method 100 for measuring viscosity temperature. The method 100 can be used, for example, with a test device. The method 100 begins at box 102, where a resin sample is screened. Screening removes agglomerates that may interfere with viscosity measurement. For example, a resin sample can be screened through a No. 12 net (with an opening of about 1.68 mm). At box 104, a measured amount of resin is added to the test device. For example, about 300 g of screened polymer resin can be added to the test device. At box 106, the test device is placed under vacuum before adding ICA (such as IC5) to ensure the correct measurement of the partial pressure of ICA. At box 108, a certain amount of ICA is added to the test device to reach the expected partial pressure. For example, using the test device, five levels are tested for each resin tested, corresponding to 0, about 25 cc, about 50 cc, about 100 cc or about 200 cc of IC5 added. At box 110, the test device is then stirred at a constant rate. For example, using the test apparatus's air-operated stirring motor, a constant nitrogen pressure of about 30 psi (about 207 kPa) is applied to maintain a constant torque.

[0097] At box 112, the reactor temperature is slowly increased until the torque limit is exceeded. For example, using a test device, when the torque limit is exceeded, the mixing motor is stopped, thereby indicating the viscosity temperature. The test is not limited to the stopping of an air-operated mixing motor. For example, a torque measuring device can be used to measure the torque applied to the test device to determine when the torque exceeds a preset target.

[0098] For most of the test, the mixer speed was essentially constant. However, as the resin began to agglomerate, the mixer speed began to slow and then stopped. The point at which the mixer speed dropped to zero was the viscosity temperature. The test was repeated at a variety of different ICA addition levels as noted above.

[0099] The viscosity temperature is related to a linear function of ICA concentration. The results from the test allow the development of a model for predicting resin viscosity temperature (T viscosity) covering the metallocene catalyst system tested. The coefficients of the linear function can be generated based on resin density, MI and MFR. Although the test resins can be made using metallocene catalysts, when the model is generated based on experience, the parameters can be adjusted for other catalyst systems, such as by repeating the model development run for those resins.

[0100] Model predictions can be verified relative to bed settling experiments carried out in a pilot plant scale gas phase fluidized bed reactor. In these experiments, non-reactive tests can be carried out to determine the temperature at which the resin agglomerates. Testing can be started by purging the drying reactor with high purity nitrogen at an elevated temperature (e.g., greater than about 75°C). The test resin sample can be passed through a 10 mesh screen (with an opening of about 0.25 mm) to remove agglomerates, and then loaded into the reactor. Using a nitrogen stream, the resin can be dried to about 10 parts per million (ppmv) of water by volume. The test resin can be heated to at least 85°C, and the reactor conditions can be adjusted to the desired ethylene partial pressure, comonomer concentration, and ICA concentration. Samples can then be collected for measuring melt flow and particle size.

[0101] The resin temperature can then be increased by about 2°C or 3°C at a rate of about 1°C per 30 minutes. Once the target temperature is reached, the temperature is stabilized for 30 minutes. The bulk density, bed weight, and surface temperature of the fluidization can be noted. The circulating compressor can then be turned off, and the bed can be allowed to settle on the distribution plate. After about 15 minutes, the circulating compressor can be turned back on to fluidize the resin. If the bed is not fluidized, the test is terminated. If the bed does fluidize, the reactor is given about five minutes to stabilize before starting the next temperature increase. Repeat this procedure until the bed agglomerates to the point where fluidization is lost.

[0102] The viscosity temperature model can be combined with the dew point calculation to define an operability window (e.g., a non-stick operating regime in a reactor operating profile) for making resins made with the metallocene catalyst being tested. Other models specific to resins made with other metallocene catalysts, Ziegler catalysts, or chromium catalysts, etc. can be generated. Since the model is based on empirical measurements of resin properties and reactor conditions, resins produced with mixtures and combinations of catalysts can also be made.

[0103] Figure 2 is a process flow diagram of a method 200 for operating a reactor in a non-stick regime. The method 200 begins at block 202, where a model of viscosity temperature is developed. Figure 1 The measured values ​​produced by the method 100 discussed are used, and the measured data are fitted to develop the parameters of equations 1-4 to develop the model. At box 204, the dew point of the ICA can be determined at each of the equivalent partial pressures of the ICA. The dew point indicates the condition of temperature and equivalent partial pressure of ICA, below which the liquid ICA begins to condense in the reactor. The formation of liquid ICA can increase the possibility of agglomeration and case operation problems by condensing in the instrumentation tap.

[0104] At frame 206, viscosity temperature and dew point can be used to identify non-stick solutions. Once a non-stick solution is established, at frame 208, ICA concentration and temperature can be adjusted to remain within a safe operation solution. For example, a new resin production run can be started at a slow initial production rate. Then ICA concentration, temperature, or both can be slowly increased to increase production rate while the reactor is maintained within a safe operation solution. If a reactor upset causes the operation to leave the non-stick solution, or indicates that stickiness may be imminent, the control system can recommend changes to force the operation to return to the non-stick solution, such as by reducing or raising the temperature, by reducing the amount of ICA returned from the recirculation system, or by injecting a kill solution for slowing down or stopping the reaction, etc. The control system can identify problematic operations before the reactor is shut down due to agglomeration.

[0105] The predicted viscosity temperature (Tviscosity) from the model can be plotted. To provide a limit, Tviscosity is adjusted to a lower value using Equation 2 to provide a safety margin. Treactor,max = Tviscosity - UT Dmax Equation 2 In Equation 2, Treactor,max represents the maximum operating temperature that can be used without significant risk of agglomeration. Dmax represents the upper temperature limit Δ that provides a buffer between the viscosity temperature measured in the experiment and the temperature at which viscosity may actually set in. Typically, a limit of 10°C below the viscosity temperature is allowed in order to operate the reactor safely. Therefore, the value of Treactor,max provides an upper temperature limit for the reactor.

[0106] The dew point (Tdew) can be plotted. Similar to the maximum operating temperature, the dew point can be adjusted using Equation 3 to provide a wider safety margin. Treactor,min = T 露 + LT Dmax Equation 3

[0107] In equation 3, LT Dmax is the lower temperature limit Δ for accounting for capillary condensation, which occurs in the reactor at about 10 °C above the actual dew point of the ICA. The value of Treactor,min provides the lower temperature limit for the reactor.

[0108] The upper and lower temperature limits define the non-sticky regime for the reactor within the drawn two-dimensional space. Another region defined by these limits is the sticky regime, where the resin begins to melt and thus becomes sticky. Other regions include the sticky + liquid regime, where both resin melting and IC5 (or other ICA) condensation are more likely to make the resin sticky. Below the upper and lower temperature limits are the liquid regimes, where IC5 (or other ICA) begins to condense and makes the resin sticky.

[0109] The current reactor conditions can be plotted by temperature and ICA equivalent partial pressure. In order to operate the reactor without agglomeration, the operator keeps the current reactor conditions within the non-stick regime. The operator can change the reactor parameters to move the reactor conditions toward the neck where the limits meet, to increase productivity, while still remaining within the non-stick regime. It can be noted that as the conditions are pushed closer to the neck, the operation becomes less flexible and the error space shrinks, making process upsets (such as temperature and concentration excursions) more problematic.

[0110] The model essentially predicts the operating window in both the pilot plant reactor and the commercial plant. The model can be used (e.g., by equations determined according to the above tests) to produce polyethylene copolymers (e.g., according to those described herein) in the following manner, for example: by increasing the ICA concentration while still remaining within the non-stick regime to set the desired operating conditions to provide the desired production rate. In addition, the model can be used to identify operations within problematic regimes and adjust reactor conditions before operational problems or shutdowns occur. Products

[0111] The polyethylene copolymers of the present disclosure may be particularly suitable for making end-use articles, such as films (e.g., such as may be formed by lamination, extrusion, coextrusion, casting and / or blow molding); and other articles such as may be formed, for example, by rotational molding or injection molding. The polyethylene copolymers may be formed into articles by cast film extrusion, blown film extrusion, rotational molding or injection molding processes. In some embodiments, the polyethylene copolymers may be used as blends.

[0112] It has been found that the polyethylene copolymers of the present disclosure can provide excellent shear thinning characteristics, while the extrudates have little or no melt fracture at high die shear rates. For example, a polyethylene copolymer having an MI of 1.5 to 2.5 and about 0.92 g / cm 3 (e.g. 0.918 to 0.921 g / cm 3 or 0.916 to 0.921 g / cm 3 ) can be used as a skin layer in a multilayer blown film to provide a film without melt fracture, thereby allowing polymer processing aids (such as perfluoroalkanes or polyfluoroalkanes) to be only optional (or preferably, completely eliminated from such blown film formulations so that the film contains no or substantially no polymer processing aids (such as fluoropolymer processing aids)). In addition, compared to other LLDPE, the polyethylene copolymers of the present disclosure (e.g., MI of 1.5 to 2.5 and density of 0.914 to 0.925 g / cm 3 , such as 0.916 to 0.921 g / cm 3) can provide films formed with reduced motor load and melt pressure (which increases input) due to improved flow behavior.

[0113] In some embodiments, the polyethylene copolymer or its blend is 80-150 s -1 The 200 Å / min thick extrudate provides a smooth extrudate at apparent die (wall) shear rates between 200 Å and 200 Å without significant melt fracture by visual observation (even in the absence of a PPA such as a fluorinated PPA).

[0114] The polyethylene copolymer (or its blend) of the present disclosure can be used in forming operations such as film, sheet and fiber extrusion and coextrusion and blow molding, injection molding and rotational molding. Film includes blow molding or cast film formed by coextrusion or by lamination, which can be used as shrink film, cling film, stretch film, sealing film, oriented film, snack packaging, heavy-duty bags, grocery bags, baking and frozen food packaging, medical packaging, industrial lining, diaphragm (membrane) etc. in food contact and non-food contact applications. Fiber includes melt spinning, solution spinning and melt-blown fiber operations for making filters, diaper fabrics, medical clothing, geotextiles etc. in woven or nonwoven forms. Extruded products include medical tubing, wire and cable coatings, pipelines, geomembranes and pond liners. Molded products include single-layer and multilayer structures in the form of bottles, cans, large hollow products, rigid food containers and toys.

[0115] Polyethylene copolymer (or its blend) can be formed into monolayer or multilayer film.These films can be formed by any conventional technique including extrusion, coextrusion, extrusion coating, lamination, blow molding and casting.Film can be obtained by flat film or tubular process, and can be oriented in the film plane in a uniaxial direction or in two mutually perpendicular directions subsequently.One or more layers of film can be oriented to the same or different degree in the horizontal and / or longitudinal direction.This orientation can occur before or after individual layers are put together.For example, polyethylene copolymer (or its blend) layer can be extrusion coated or laminated on oriented polypropylene layer, or polyethylene copolymer (or its blend) and polypropylene can be coextruded into film together, then oriented.Similarly, oriented polypropylene can be laminated to oriented polyethylene copolymer (or its blend), or oriented polyethylene copolymer (or its blend) can be coated on polypropylene, then optionally can even further oriented this combination.

[0116] Films include monolayer or multilayer films. Specific end-use films include, for example, blown films, cast films, stretch films, stretch / cast films, stretch cling films, stretch hand wrap films, machine stretch wrap, shrink films, shrink wrap films, greenhouse films, laminates, and laminated films. Exemplary films are prepared by any conventional technique known to those skilled in the art, such as, for example, techniques for preparing blown, extruded, and / or cast stretch and / or shrink films (including shrink-shrink applications).

[0117] In one embodiment, multilayer film (multilayer film) (multilayer film (multilayer-layer film)) can be formed by any suitable method.The total thickness of multilayer film can vary based on the desired application.5-100 μm, such as 10-50 μm total film thickness is suitable for most applications.It will be appreciated by those skilled in the art that the thickness of the individual layers of multilayer film can be adjusted based on the desired end-use performance, the polymer adopted, the equipment capacity and other factors.The material forming each layer can be coextruded by a coextrusion feedblock and a die assembly to produce a film having two or more layers that adhere together but have different compositions.Coextrusion can be applicable to both cast film and blown film processes.Exemplary multilayer films have at least two, at least three or at least four layers.In one embodiment, multilayer film is composed of five to ten layers. Example Example 1

[0118] Several experiments were conducted in a gas phase fluidized bed polymerization reactor to explore new combinations of melt index and density to understand product properties.

[0119] A combination of resin properties was selected as a suitable candidate for commercial scale shaping. Historical modeling calculations were performed using a method based on the manufacturing reactor environment. The results of the initial calculations determined were at high risk of discontinuity in the commercial reactor environment. Without further information, these modeling calculations alone may result in project interruption. However, a new T viscosity model for this type of metallocene-catalyzed LLDPE was also applied to calculate continuity risk, thereby acting as an additional check on traditional modeling. It was then determined that the risk was not as high as initially expected, which led to additional pilot plant testing. Further experiments were performed on the pilot scale reactor to understand the full product performance at different temperatures, as temperature may be a factor causing poor continuity and viscosity.

[0120] The polyethylene copolymers according to one or more embodiments provided herein are produced in a gas phase polymerization system. The properties of the inventive resins are shown in Table 1.

[0121] Inventive resins I1, I2, I3, I4, I5 and I13 were produced on a pilot plant scale; inventive resin I8 was produced on a commercial scale.

[0122] Polymerization is carried out in a continuous gas phase fluidized bed reactor. Polymerization conditions are shown in Table 2 below. The fluidized bed consists of a catalyst and growing polymer particles. The gaseous feed stream of ethylene and hydrogen is mixed with the liquid comonomer in a mixing tee arrangement and introduced into the recycle gas production line below the reactor bed. ICA (isopentane) is added together with ethylene and hydrogen and also introduced into the recycle gas production line below the reactor bed. The individual flow rates of ethylene, hydrogen and comonomer are controlled to maintain a fixed composition target. The ethylene concentration is controlled to maintain a constant ethylene partial pressure. Hydrogen is controlled to maintain a constant hydrogen to ethylene molar ratio. The concentration of each gas is measured by an online gas chromatograph to ensure that the composition in the recycle gas stream is relatively constant.

[0123] Business Enable TM 2010 polyethylene grades exhibit flow challenges in dies and extruders used in cast film lines, resulting in high melt pressures, high motor loads, and suboptimal flow to the die mid-edge, which can cause encapsulation of adjacent resin layers. Figure 1 As shown in , the resin of the present invention is outside the Enable window of MI and density. Figure 1 As shown in the table, "Enable" refers to various ENABLEs available from ExxonMobil Chemical Company in Houston, TX. TM Resin Grades. "XP 6000" is a series of resins available from ExxonMobil Chemical Company, Houston, Texas. I8 is an example of a resin of the present invention.

[0124] Discover I8 Resin and ENABLE TM The higher melt index compared to 2010 improves flow behavior and improves process limitations. It is found that lower density (e.g. 0.916 g / cm 3 and 0.918 g / cm 3 ) improves film properties such as puncture resistance; achieving such improved (ie, higher) puncture resistance improves package consistency and can improve holding force on the pallet during shipping.

[0125] In addition, in commercial ENABLE TMThe presence of a small amount of long chain branching (LCB) in the grade can improve the processability in cast film applications. The presence of LCB generally provides processing advantages, such as reduced shrink-in and increased tensile stability. It is found that the inventive resin of the present disclosure can maintain such favorable LCB, even while achieving improved density and MI, thereby unexpectedly achieving an acceptable production rate suitable for a commercial process. In addition, the lower zero shear viscosity of the inventive resin can result in lower discharge pressures and temperatures in the extrusion process, thereby resulting in increased output, compared to the comparative commercial grades. Table 1.1 : Analytical data of resins I1-I8 of the present invention Table 1.2 : Analytical data of resins I9-I13 of the present invention Table 1.3 : Analytical data of comparative resins C1-C7 Table 2 : Process conditions of some embodiments of the present invention

[0126] Figure 4A : is the gel permeation chromatography chromatogram of the resin of the present invention and the comparative resin. Figure 4A As shown in , the traces for the inventive resins show similar average molecular weight and MWD as the commercial resins. All of the inventive samples show evidence of LCB, with similar levels of LCB seen in the g' values.

[0127] Figure 4B is a graph showing density versus EEE triad content for inventive resins and comparative resins according to embodiments. Figure 4B The inventive resins are shown to have a unique combination of density and EEE triad content compared to comparative commercial resins.

[0128] Viscosity flow data using SAOS data are shown in Figure 5The viscosities of the inventive resins and comparative resins at about 100 rad / s (η100) and 0.01 rad / s (η0.01) are shown in Table 1. During the extrusion stage of film manufacturing, shear rates approaching 100 to 1000 rad / s are typically encountered. I8 and C1 (ENABLE TM 2010ME) exhibit similar viscosities over a typical shear rate range for extrusion processes (approximately 30-300 rad / s), and differ more at lower shear rates near zero in determining the starting torque. I8 has a viscosity significantly lower than that of C1, and is therefore expected to involve lower screw torque for the initial extrusion process. In fact, Table 3 (below) shows the overall lower melt pressure and motor load achieved when processing I8 compared to C1.

[0129] Return to reference Figure 5 All of the inventive resins showed significantly lower η compared to the comparative resins. 0.01 It should be understood that in ENABLE TM The presence of a small amount of long chain branching (LCB) in the grade improves processability in cast film applications. The lower viscosity (at a low shear rate of 0.01 rad / s) of the resin of the present invention compared to commercial grades can result in lower discharge pressures and temperatures during extrusion, which can result in increased production. LCBs generally result in processing advantages such as reduced shrink-in and increased tensile stability.

[0130] Business Enable TM Grades (C1-C4) contain LCB which not only positively impacts processability but also results in unique film properties. Therefore, it is desirable that some embodiments maintain a critical level of LCB so as not to affect those film properties. Figure 6 VGP (Van Gurp Palmen) curves for the inventive resins and comparative commercial resins are shown. All inventive grades show an inflection point in the curve indicating the presence of LCB. TM XP 8318 (LLDPE without such LCB) is included as a comparison of the VGP curves of LLDPE without any LCB. Figure 6 Thus, the polyethylene copolymers of the present disclosure may be characterized as having an inflection point in the Van Gurp Palmen curve.

[0131] The comonomer distribution in the comparative grade and the inventive grade was determined based on the TREF results. Figure 7It is shown that the peak elution temperature decreases with increasing amount of comonomer in the sample. Compared to C1, C2 and C4, I8 has the lowest peak temperature. The width of the distribution also increases with increasing amount of comonomer when compared to C1, C2 and C4, with I8 showing a significantly wider chemical composition distribution.

[0132] Figure 8 is a graph showing the melt strength of I8 and C14. At 190°C, the melt strength of I8 is about half of that of C1. Example 2

[0133] Fig. 9 A radar chart is shown comparing melt pressure, melt temperature and motor load for making films on a casting line using I8 or C1 (using the same operating conditions for I8-based cast films and C1-based cast films). Table 3 shows the corresponding extruder variables for I8 and C1 related to this example. Table 3 : Extruder parameters of I8 and C1 during cast film manufacturing. I8 C1 Melt pressure (bar) 190 252 Melt temperature(℃) 286 287 Motor load (%) 36 39 Example 3

[0134] Fig.10 A similar radar chart is shown comparing the melt pressure, melt temperature and motor load generated by making blown film on a 5-layer line using I2 or C1. Table 4 shows the melt pressure, melt temperature and motor load generated by making blown film on a 5-layer line using I2 or C1. Fig.10 The Example 3 manufacturing data depicted in FIG. 1 is related to the corresponding extruder variables of I2 and C1. Table 4 : Extruder parameters of I2 and C1 in blown film manufacturing process I2 C1 Melt pressure (bar) 321 363 Melt temperature(℃) 204 206 Motor load (%) 45 50 Example 4

[0135] In another experiment, blown films were made on a Wild Hall (W&H) 5-layer blown film line. In one embodiment, I2 was used as the skin layer, and a LLDPE with essentially no long chain branching, produced using a pair of metallocene catalysts and having a broad orthogonal composition distribution was used as the core layer ("2-catalyst LLDPE"). The density of this LLDPE was 0.920 g / cc and the MI was 0.80 g / 10 min. This LLDPE did not contain any PPA. Table 5.1 shows the film line parameters; Table 5.2 shows the process parameters of each extruder used in the coextrusion blown film production. Table 5.1 : Blown film parameters of Example 4 parameter value Die head diameter 280mm Die gap 1.4mm Target thickness 50μm BUR (Blowing Ratio) 2.5 Frost line height 850mm Production line speed 37.2m / min Table 5.2 : Example 4 Extrusion process parameters Example 5

[0136] In another example, I3 was used in the same blown film line with the same parameters as in Table 5.1 above (except that the line speed was 37.1 m / min instead of 37.2 m / min). I3 was used as the skin layer, and the same 2-catalyst LLDPE as in Example 4 was used as the core layer ("2-catalyst LLDPE"). The density of this LLDPE was 0.920 g / ml and the MI was 0.80 g / 10 min. This LLDPE did not contain any PPA.

[0137] The operating conditions of the extruder of Example 5 are described in Table 6. Table 6 : Example 5 Extrusion process parameters Example 6

[0138] Finally, a comparative 5-layer blown film process was performed with the same film line parameters as in Table 5.1. A slightly different dual-catalyst LLDPE was used as the core layer (2-catalyst LLDPE-2) with a density of 0.926 g / cc and a MI of 0.85 g / 10 min; and ENABLE TM 2010(C1), Exceed TM 3812 and / or LD150 made the other layers as indicated in Table 7 below. Table 7 shows the extruder processing parameters for the 5-layer blown film line associated with this Example 6.

[0139] Although the core is slightly different from Examples 4 and 5, the key comparison here is the processing of commercial resins in a separate extruder compared to the I2 (Example 4) or I3 (Example 5) resins above, where the superior processability of I2 and I3 compared to the commercial resins can be quickly seen. In addition, it is important to note that the Example 4 and 5 blown films were made without the use of a polymer processing aid (PPA), and no melt fracture was observed in those films. In contrast, melt fracture is typically seen when resins without processing aids are used. On the other hand, melt fracture was observed when C1 was used. Table 7 : Comparison of extrusion process parameters of blown film embodiment 6 1 2-Catalyst LLDPE resin (D = 0.926 g / cc, MI = 0.85 g / 10 min) 2 EXCEED TM 3812 resin is available from ExxonMobil Chemical Company in Houston, Texas. 3 LD 150 resin is available from ExxonMobil Chemical Company, Houston, Texas.

[0140] It was observed that approximately 20% reduction in melt pressure was obtained with the inventive resin compared to the comparative resin, thereby providing increased throughput in film production. In addition, the observed improvement in flow to the edge provided a functional layer that could be used as a skin layer. A 10% reduction in motor load was also observed with the inventive resin.

[0141] In general, polyethylene polymers, polymerization processes for making such polyethylene polymers, and films made from such polyethylene polymers offer many advantages. The polyethylene polymers may be copolymers having a combination of low density, high melt index, retention of long chain branching, and relatively consistent comonomer incorporation (high CDBI) across polymer chains of varying lengths, while also providing commercially desirable polymerization and extrusion of polyethylene copolymers.

[0142] Certain embodiments and features have been described using a set of numerical upper limits and a set of numerical lower limits. It should be understood that, unless otherwise indicated, ranges including combinations of any two values ​​are contemplated, such as any lower value combined with any higher value, any two lower values ​​combined, and / or any two higher values ​​combined. Certain lower limits, upper limits, and ranges appear in one or more of the claims below. All numerical values ​​are "about" or "approximately" indicated values, and take into account experimental errors and variations that would be expected by a person of ordinary skill in the art.

[0143] All priority documents are fully incorporated herein by reference for all purposes and in all jurisdictions that allow such incorporation and to the extent such description is consistent with the present disclosure. In addition, all documents and references cited herein (including test procedures, publications, patents, journal articles, etc.) are fully incorporated herein by reference in all jurisdictions that allow such incorporation and to the extent such description is consistent with the present disclosure.

[0144] Likewise, whenever a composition, element, or group of elements is preceded by the transition phrase "comprising," it is understood that we also contemplate the same composition or group of elements preceded by the transition phrases "consisting essentially of," "consisting of," "selected from the group consisting of," or "is," and vice versa. Unless otherwise stated, the phrases "consist essentially of and consisting essentially of" do not exclude the presence of other steps, elements, or materials, whether or not specifically mentioned in the specification, as long as such steps, elements, or materials do not affect the basic and novel characteristics of the claimed invention, and further, these phrases do not exclude impurities and variations normally associated with the elements and materials used.

[0145] Although the claimed invention has been described with respect to several embodiments and examples, those skilled in the art, having benefit of this disclosure, will appreciate that other embodiments can be devised which do not depart from the scope and spirit of the disclosure.

Claims

1. A polyethylene copolymer comprising: Ethylene units; and 1 wt% to 8 wt% of C3-C8 α-olefin comonomer units, the polyethylene copolymer having: 0.914g / cm 3 Up to 0.925g / cm 3 The density of a melt index (MI, determined according to ASTM D1238 at 190° C. and 2.16 kg load) greater than 1 g / 10 min and less than or equal to 2.5 g / 10 min, A composition distribution breadth index of 75% or greater, and 2 to 8 molecular weight distribution (M w / M n ).

2. The polyethylene copolymer of claim 1 having long chain branching.

3. The polyethylene copolymer of claim 1 or claim 2, having one or more of the following: (i) a melt index ratio (MIR) in the range of 25 to 40, wherein MIR is the ratio of the high load melt index (HLMI, ASTM D1238, at 190°C, 21.6 kg) to the melt index (MI, ASTM D1238, at 190°C, 2.16 kg); (ii) an inflection point in a Van Gurp Palmen plot of phase angle versus complex modulus (Pa) of the polyethylene copolymer; and (iii) a shear thinning ratio of less than 15.

4. A polyethylene copolymer as claimed in any one of the preceding claims, wherein The polyethylene copolymer has a Q parameter of 50 to 90 as determined by equation (1): Q parameter = 0.001*(MIR*η 0.01 / η 100 ) 2 *(T 75 -T 25 ) / MWD (Equation 1) Where MIR is the melt index ratio, η 0.01 is the complex shear viscosity (η*) at 0.01 rad / s and 190°C, η 100 is the complex shear viscosity (η*) at 100 rad / s and 190°C, T 75 -T 25 It is T 75 -T 25 Value, where T 25 is the temperature and T at which 25% of the polyethylene copolymer is eluted using the temperature-increasing elution fractionation. 75 is the temperature at which 75% of the polyethylene copolymer is eluted using rising temperature elution fractionation, and MWD is the molecular weight distribution.

5. A polyethylene copolymer as claimed in any one of the preceding claims, wherein The polyethylene copolymer has 0.1 to 0.15 tri-substituted vinylene groups per 1000 carbon atoms.

6. A polyethylene copolymer as claimed in any one of the preceding claims, wherein The polyethylene copolymer has an [EEE] triad content of 89 mol% to 91.8 mol%.

7. A polyethylene copolymer as claimed in any one of the preceding claims, wherein The polyethylene copolymer has: 3 mol% to 8 mol% [HEE] triad content, 0.05 mol% to 0.5 mol% [HEH] triad content, 1 mol% to 5 mol% [EHE] triad content, 0.05 mol% to 0.5 mol% [EHH] triad content, and 0.05 mol% to 0.5 mol% [HHH] triad content.

8. A polyethylene copolymer as claimed in any one of the preceding claims, wherein The polyethylene copolymer has a thickness of 0.918 g / cm 3 Up to 0.922g / cm 3 density.

9. A polyethylene copolymer as claimed in any one of the preceding claims, wherein The polyethylene copolymer has a thickness of 0.915 g / cm 3 Up to 0.920g / cm 3 density.

10. The polyethylene copolymer according to claim 1, wherein The C3-C8 alpha-olefin comonomer unit is a 1-hexene unit, and the polyethylene copolymer comprises 92 wt% to 99 wt% ethylene.

11. A polyethylene copolymer as claimed in any one of the preceding claims, wherein The polyethylene copolymer further has one or more of the following characteristics: (a) MI of 1.5 g / 10 min to 2.3 g / 10 min; (b) T between 4°C and 10°C 75 -T 25 value; (c) a high load melt index (HLMI, determined according to ASTM D1238 at 190° C. and 21.6 kg load) of 45 to 70 g / 10 min; (d) a melt index ratio (MIR, HLMI / MI) of 27 to 33; (e) a weight average molecular weight (Mw) of 70,000 g / mol to 95,000 g / mol; or (f) a number average molecular weight (Mn) of 20,000 g / mol to 40,000 g / mol.

12. The polyethylene copolymer of claim 11, having all of the properties (a) to (f).

13. The polyethylene copolymer according to any one of claims 1 to 12, wherein The polyethylene copolymer has a HLMI of 45 g / 10 min to 55 g / 10 min.

14. The polyethylene copolymer according to any one of claims 1 to 12, wherein The polyethylene copolymer has a HLMI of 60 to 70 g / 10 min.

15. The polyethylene copolymer according to any one of claims 1 or 2 to 14, wherein The polyethylene copolymer has: a complex shear viscosity (η*) at 0.01 rad / s and 190° C. of 6,000 Pa·s to 8,000 Pa·s, and Complex shear viscosity (η*) at 100 rad / s and 190° C. of 1,100 Pa·s to 1,300 Pa·s.

16. A cast film comprising a polyethylene copolymer as claimed in claim 1 or any one of claims 2 to 14, wherein: The polyethylene copolymer has a thickness of 0.915 g / cm 3 Up to 0.917g / cm 3 The density and melt index of 1.6 g / 10 min to 1.8 g / 10 min.

17. A blown film comprising the polyethylene copolymer of claim 1 or any one of claims 2-14, wherein The polyethylene copolymer has a thickness of 0.918 g / cm 3 Up to 0.922g / cm 3 The density and melt index of 1.5 g / 10 min to 2.3 g / 10 min.

18. The blown film of claim 17, wherein The blown film is substantially free of perfluoroalkanes or polyfluoroalkanes.

19. A method comprising: measuring a viscosity temperature of the polyethylene copolymer at each of a plurality of concentrations of an inducing condensation agent in a test apparatus; measuring the density, melt index (MI) and high load melt index (HLMI) of the polyethylene copolymer; Calculating a melt flow ratio by dividing the HLMI by the MI; calculating an equivalent partial pressure of the induced condensing agent, the equivalent partial pressure corresponding to the partial pressure of the isomer accumulated in the reactor; and determining an equation relating the viscosity temperature to the equivalent partial pressure based at least in part on the density, MI, and MFR of the polyethylene copolymer, and Using the equation, an additional amount of the polyethylene copolymer is produced, wherein the polyethylene copolymer comprises: Ethylene units; and 1 wt% to 8 wt% of C3-C8 α-olefin comonomer units, the polyethylene copolymer having: 0.914g / cm 3 Up to 0.925g / cm 3 The density of a melt index (MI, determined according to ASTM D1238 at 190° C. and 2.16 kg load) greater than 1 g / 10 min and less than or equal to 2.5 g / 10 min, A composition distribution breadth index of 75% or greater, and 2 to 8 molecular weight distribution (M w / M n ).

20. A method for producing a polyethylene copolymer as claimed in any one of claims 1 to 15, the method comprising: measuring one or more parameters of the polymerization reaction, the one or more parameters comprising reactor temperature and a concentration of an induced condensing agent (ICA) in the polymerization reactor; Calculating the equivalent partial pressure of the ICA; positioning the polymerization reaction in two dimensions on a map defined by a reactor temperature dimension and an equivalent partial pressure dimension; comparing the position of the polymerization reaction in the two-dimensional space to a no-stick regime, the no-stick regime being defined as the space between an upper temperature limit curve and a lower temperature limit curve; adjusting the one or more parameters of the polymerization reaction to operate the polymerization reaction within the non-stick regime; as well as Based on the adjusted one or more parameters, the polyethylene copolymer according to any one of claims 1 to 15 is obtained from the polymerization reactor.

Citation Information

Cited By

  • High performance polyethylene film with improved aging properties

    CN119795718A