Cerium-doped bismuth germanate scintillation ceramic material as well as preparation method and application thereof
By doping cerium in BGO, Bi4Ge3O12:xCe material is formed, which solves the problems of excessive BGO light output and poor radiation resistance, and reduces light output and improves radiation resistance, shortens attenuation time, and is suitable for high-energy Radiation detection applications of physical and large scientific installations.
Patent Information
- Application Number
- CN202310590418.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-24
AI Technical Summary
BGO scintillator has too high light output in high-energy physics and large scientific devices, resulting in signal saturation, and has poor stability in high-radiation environments, and its long attenuation time limits the application of high-counting rate radiation detection, and radiation damage affects uniform light response sex.
By doping cerium (Ce) into BGO, Bi4Ge3O12:xCe material is formed, and Ce4+ and Ce3+ account for 70-80% and 20-30% respectively, to reduce light output, improve radiation resistance and shorten attenuation time.
It significantly reduces the light output of BGO, improves radiation resistance, shortens attenuation time, improves scintillation characteristics, and is suitable for the radiation detection field of high-energy physics and large scientific devices.
Smart Images

Figure CN119019164A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cerium-doped bismuth germanate scintillation ceramic material and a preparation method and application thereof, belonging to the field of scintillators for radiation detection. Background Art
[0002] Scintillators are a type of functional material that can absorb the energy of high-energy particles or radiation and convert it into ultraviolet-visible or near-infrared photons, which are then converted into electrical signals through photodetectors such as photomultipliers and silicon photomultipliers (SiPMs), thereby accurately detecting and identifying the type, quantity, energy, direction and position of incident high-energy particles or rays. Scintillator-based scintillation detectors have been widely used in high-energy physics, medical imaging, security inspection, resource exploration, environmental monitoring and industrial testing.
[0003] Doping is a reliable means to improve and improve the deficiencies of existing scintillating materials. With the differentiated needs of radiation detection, while researching and developing new scintillators with better performance, people have been trying to improve the scintillation performance of existing materials with large-scale manufacturing capabilities through doping, such as calcium-cerium co-doping to shorten the decay time of lutetium silicate crystals and enhance their light output (MASpurrier et al., Effects of Ca2+). 2+ Co-Doping on the Scintillation Properties of LSO: Ce, IEEE Trans. Nucl. Sci., 55 (2008): 1178-1182), yttrium doping suppresses the slow scintillation component in barium fluoride scintillation crystals, which has a light output 4-5 times that of the fast scintillation component (J. Chen et al., "Slow Scintillation Suppression in Yttrium Doped BaF2 Crystals," IEEE Trans. Nucl. Sci. 65 (2018): 2147-2151), fluorine doping improves the light output of lead tungstate scintillation crystals, and yttrium doping improves its light transmittance and photoresponse uniformity (Wang Shaohua, Macroscopic defects in lead tungstate crystals and their doping effects, doctoral dissertation of Shanghai Institute of Ceramics, Chinese Academy of Sciences, 1999).
[0004] Bismuth germanate (Bi4Ge3O 12 , BGO) crystal is an inorganic scintillator with excellent comprehensive performance and high density (7.13g / cm 3 ), large effective atomic number (Z eff, 74), with outstanding advantages such as strong radiation blocking ability, high detection efficiency, moderate energy resolution, large intrinsic peak / comon ratio, good uniformity, no luminescent self-absorption, no afterglow, stable physical and chemical properties and good machinability, it has extensive and important applications in high-energy physics, astrophysics, nuclear physics, nuclear medical imaging, geological exploration, oil well logging and industrial detection. Since the 1980s, the crystal has been mass-produced, and with the deepening of research and development, there have been continuous breakthroughs in size and performance. It is still one of the most important and largest-scale inorganic scintillators. The Circular Electron Positron Collider (CEPC) and the Future Circular Collider (FCC) are large scientific facilities at the forefront of intensity, and the beam intensity is significantly higher than that of the existing Large Hadron Collider (LHC) and other devices, which puts higher requirements on the hardness and time response characteristics of scintillating crystals.
[0005] Silicon photomultiplier (SiPM) is a new type of highly sensitive semiconductor photodetector device, which consists of an array of multiple pixels connected in parallel in Geiger mode. Each pixel is composed of an avalanche photodiode and a quenching resistor in series. SiPM has the characteristics of high quantum efficiency, high gain, good signal-to-noise ratio, fast time response, low operating voltage, magnetic field insensitivity and compact structure. It has become the preferred scintillation photodetector device for devices such as CEPC and FCC, and is also the preferred choice for light readout of various scintillation detectors. Due to the large number of scintillation photons generated by GeV-TeV high-energy particles, when all pixels detect photons at the same time, the output signal of SiPM will be saturated, that is, there are no more pixels available to detect other incident photons, which will directly affect the dynamic range and accuracy of the electric energy device. Although the light output of the crystal can be reduced by attenuation plates, its stability and reliability in strong radiation environments cannot be guaranteed. Therefore, it is urgent to reduce the light output of BGO crystals to better meet the urgent application needs of large scientific facilities such as CEPC and FCC.
[0006] In addition, after being exposed to a certain dose of high-energy particles, rays or ultraviolet radiation, the BGO crystal will flicker and its light performance will decay due to coloring, which will in turn affect the crystal's light output and light response uniformity. This is called "irradiation damage." How to reduce the radiation damage effect has always been one of the important research and development directions of BGO crystals. In addition, BGO crystals have a long decay time of ~0.3μs, which limits their application in high-count rate radiation detection such as high-energy physics and resource exploration. How to shorten their decay time has also received continuous attention. Summary of the invention
[0007] To this end, the object of the present invention is to provide a cerium-doped bismuth germanate scintillating ceramic material and a preparation method and application thereof that can reduce the light output of a BGO scintillator, improve its radiation resistance and shorten its decay time.
[0008] In a first aspect, the present invention provides a cerium-doped bismuth germanate scintillation ceramic material, wherein the chemical formula of the cerium-doped bismuth germanate scintillation ceramic material is Bi4Ge3O 12 :xCe, wherein 0<x≤0.1. Preferably, the Ce element is Ce 3+ and Ce 4+ The Ce 4+ Ce accounts for 70-80% of the total Ce element. 3+ The sum of the two is 100%. Preferably, when x=0.03, Ce 4+ 76% 3+ Accounting for 24%.
[0009] In the present disclosure, after cerium doping BGO, trivalent Ce 3+ and tetravalent Ce 4+ Two forms exist in BGO scintillator, due to and The ionic radius is much larger than The ionic radius, The ionic radius is slightly larger than that of Ce 3+ and Ce 4+ According to the general principle that the doped ions must have ionic radii similar to those of the substituted ions in the matrix lattice, after Ce ion doping, it will occupy the Bi 3+ ions in the lattice. Moreover, the irradiation change of Ce ions can inhibit the radiation in Bi4Ge3O 12 The formation of color centers caused by 12 In addition, the present invention reduces the light output of BGO by Ce doping, which not only inhibits radiation damage but also shortens its decay time, which has important research significance and practical value.
[0010] Preferably, x=0.01-0.05, preferably 0.02-0.04, more preferably 0.03.
[0011] Preferably, the cerium-doped bismuth germanate scintillating ceramic material is in the form of ceramic powder, preferably with a particle size of 50 nm to 50 μm.
[0012] Preferably, the cerium-doped bismuth germanate scintillating ceramic material is in the form of a ceramic block.
[0013] In a second aspect, the present invention provides a method for preparing a bismuth cerium germanate scintillation ceramic material, wherein the chemical formula of the bismuth cerium germanate scintillation ceramic material is Bi 4-x Ge3O 12 : xCe, where 0<x≤0.1; The cerium-doped bismuth germanate scintillation ceramic material is in the form of ceramic powder, and the preparation method comprises: (1) According to the chemical formula of cerium-doped bismuth germanate scintillating ceramic material Bi4Ge3O 12 :xCe weigh Bi source, Ge source and Ce source and mix them to obtain a mixed powder; (2) Sintering the mixed powder at 800-900° C. for 1-10 hours to obtain the cerium-doped bismuth germanate scintillating ceramic material.
[0014] Preferably, the Bi source is Bi2O3; the Ge source is GeO2; and the Ce source is at least one of CeO2, Ce2O3, CeF3, and Ce(NO3)3.
[0015] Preferably, the sintering atmosphere is air atmosphere, oxygen atmosphere or reducing atmosphere; the reducing atmosphere is a mixture of inert atmosphere and hydrogen, and the hydrogen content does not exceed 10 vol%.
[0016] In a third aspect, the present invention provides a method for preparing a bismuth cerium germanate scintillation ceramic material, wherein the chemical formula of the bismuth cerium germanate scintillation ceramic material is Bi 4-x Ge3O 12 : xCe, where 0<x≤0.1; The cerium-doped bismuth germanate scintillation ceramic material is in the form of a ceramic block, and the preparation method comprises: (1) According to the chemical formula of cerium-doped bismuth germanate scintillating ceramic material Bi4Ge3O 12 :xCe weigh Bi source, Ge source and Ce source and mix them to obtain a mixed powder; (2) pressing the mixed powder into a shape to obtain a ceramic green body; (3) The ceramic green body is subjected to hot pressing or hot isostatic pressing to obtain the cerium-doped bismuth germanate scintillating ceramic material.
[0017] Preferably, the Bi source is Bi2O3; the Ge source is GeO2; and the Ce source is selected from at least one of CeO2, Ce2O3, CeF3, and Ce(NO3)3.
[0018] Preferably, the parameters of the hot pressing sintering include: pressure of 0.03-5 GPa, sintering temperature of 500-900°C, and sintering time of 1-20 hours; The parameters of the hot isostatic pressing sintering include: a pressure of 0.03 to 5 GPa, a sintering temperature of 500 to 900° C., and a sintering time of 1 to 20 hours.
[0019] In a fourth aspect, the present invention provides an application of a cerium-doped bismuth germanate scintillating ceramic material in the field of radiation detection, wherein the radiation detection field includes high energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection and industrial detection.
[0020] Beneficial effects of the present invention: The present invention can reduce the light output of BGO scintillating ceramic materials by cerium doping, improve their radiation resistance, and shorten their decay time, which can significantly improve the scintillation characteristics of BGO. The present invention also provides an application of cerium-doped bismuth germanate (BGO:Ce) scintillating ceramic materials in radiation detection fields including but not limited to high energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection, industrial detection, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 1 is the X-ray diffraction pattern (XRD) of the cerium-doped bismuth germanate ceramic powder in Examples 1-5, and the standard X-ray diffraction spectrum of the bismuth germanate crystal phase is inserted at the bottom of the figure.
[0022] Figure 2 In the figure, a is the emission spectrum diagram of Example 1 before and after irradiation and the corresponding integrated area, and b is the X-ray excitation emission spectrum of Example 1 before and after irradiation and the corresponding integrated area.
[0023] Figure 3 In the figure, a is the emission spectrum diagram of Example 4 before and after irradiation and the corresponding integrated area, and b is the X-ray excitation emission spectrum of Example 4 before and after irradiation and the corresponding integrated area.
[0024] Figure 4 a is the X-ray photoelectron spectrum of Ce 3d in Example 4 before irradiation, and b is the X-ray photoelectron spectrum of Ce 3d in Example 4 after irradiation.
[0025] Figure 5 Figure a is the emission spectra of bismuth germanate ceramic powders doped with different cerium concentrations in Examples 1-6, and figure b is the comparison of the corresponding spectral integral areas.
[0026] Figure 6 The excitation spectra of bismuth germanate ceramic powder doped with different cerium concentrations in Examples 1-5.
[0027] Figure 7 These are X-ray excitation emission spectra of bismuth germanate ceramic powders doped with different cerium concentrations in Examples 1-5.
[0028] Figure 8 This is the fluorescence decay curve of Example 1 (the monitoring wavelength is 467 nm).
[0029] Fig. 9This is the fluorescence decay curve of Example 4 (the monitoring wavelength is 467 nm). DETAILED DESCRIPTION
[0030] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0031] The following is an exemplary description of the preparation method of cerium-doped bismuth germanate ceramics.
[0032] Bi source, Ge source and Ce source are used as raw materials, and are weighed according to the weight determined by the doping amount and then mixed to obtain a mixed powder. Preferably, the Bi source, Ge source and Ce source are Bi2O3, GeO2 and CeO2 respectively.
[0033] The mixed powder is sintered at 800-900° C. in air / reducing atmosphere for 1-10 hours to obtain a cerium-doped bismuth germanate powder scintillator.
[0034] The following is an exemplary description of a method for preparing a cerium-doped bismuth germanate ceramic scintillator.
[0035] Bi2O3 and GeO2 are used as raw materials, and one or a mixture of two or more oxides or chemicals such as CeO2, Ce2O3, CeF3, Ce(NO3)3 are used as dopants. After weighing according to the weight determined by the doping amount, they are mixed to obtain a mixed powder.
[0036] After the mixed powder is pressed into a shape, it is sintered at 500-900° C. for 1-20 hours in a hot isostatic press or a hot pressing furnace to obtain a cerium-doped bismuth germanate ceramic scintillator.
[0037] In the present invention, the application of the cerium-doped bismuth germanate scintillator includes, but is not limited to, radiation detection fields such as high energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection, and industrial detection.
[0038] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0039] Example 1 Take commercially available Bi2O3 and GeO2 powders as raw materials, weigh them in a molar ratio of 2:3 (x=0). Grind and mix them evenly in an agate mortar, put the mixed powders into a corundum crucible, cover it, place it in a high-temperature furnace, and sinter it at 900℃ in an air atmosphere or a reducing atmosphere (95% argon + 5% hydrogen) for 6 hours. After cooling and proper grinding, Bi4Ge3O 12 Ceramic powder.
[0040] Example 2 Take commercially available Bi2O3, GeO2, and CeO2 powders as raw materials, weigh them in a molar ratio of 1.9975:3:0.005 (0.005). Grind and mix them evenly in an agate mortar, put the mixed powders into a corundum crucible, cover it, place it in a high-temperature furnace, and sinter it at 900°C in an air atmosphere or a reducing atmosphere (95% argon + 5% hydrogen) for 6 hours. After cooling and proper grinding, Bi 3.995 Ge3O 12 :0.005Ce ceramic powder.
[0041] Example 3 Take commercially available Bi2O3, GeO2, CeO2 powder as raw materials, weigh them in a molar ratio of 1.995:3:0.01 (x=0.01). Grind and mix them evenly in an agate mortar, put the mixed powder into a corundum crucible, cover it, place it in a high-temperature furnace, and sinter it at 900℃ in an air atmosphere or a reducing atmosphere (95% argon + 5% hydrogen) for 6 hours. After cooling and grinding appropriately, Bi 3.99 Ge3O 12 :0.01Ce ceramic powder.
[0042] Example 4 Take commercially available Bi2O3, GeO2, CeO2 powder as raw materials, weigh them in a molar ratio of 1.985:3:0.03 (x=0.03). Grind and mix them evenly in an agate mortar, put the mixed powder into a corundum crucible, cover it, place it in a high-temperature furnace, and sinter it at 900℃ in air atmosphere or reducing atmosphere (95% argon + 5% hydrogen) for 6 hours. After cooling and proper grinding, Bi 3.97 Ge3O 12 :0.03Ce ceramic powder.
[0043] Example 5 Take commercially available Bi2O3, GeO2, and CeO2 powders as raw materials, weigh them in a molar ratio of 1.975:3:0.05 (x=0.05). Grind and mix them evenly in an agate mortar, put the mixed powders into a corundum crucible, cover it, place it in a high-temperature furnace, and sinter it at 900°C in an air atmosphere or a reducing atmosphere (95% argon + 5% hydrogen) for 6 hours. After cooling and proper grinding, Bi 3.95 Ge3O 12 :0.05Ce ceramic powder.
[0044] Example 6 Take commercially available Bi2O3, GeO2, and CeO2 powders as raw materials, weigh them in a molar ratio of 1.95:3:0.1 (x=0.1). Grind and mix them evenly in an agate mortar, put the mixed powders into a corundum crucible, cover it, place it in a high-temperature furnace, and sinter it at 900°C in an air atmosphere or a reducing atmosphere (95% argon + 5% hydrogen) for 6 hours. After cooling and proper grinding, Bi 3.9 Ge3O 12 :0.1Ce ceramic powder.
[0045] Example 7 Commercially available Bi2O3, GeO2, and CeO2 powders were used as raw materials and weighed in a molar ratio of 1.985:3:0.03 (x=0.03). The mixture was ground and mixed evenly in an agate mortar to obtain a mixed powder. The mixed powder was pressed into a shape and sintered in a hot isostatic pressing furnace for 6 hours at a sintering temperature of 900°C to obtain Bi2O3. 3.97 Ge3O 12 :0.03Ce ceramic block.
[0046] Figure 1 is the XRD diffraction phase analysis result of polycrystalline powder. When the doping concentration x≤0.03, the XRD diffraction peak of the powder is similar to that of Bi4Ge3O 12 The standard diffraction peaks of the main crystalline phase correspond well, and no other impurity phases are observed. In addition, when the doping concentration is higher than 0.03, the present invention observes the presence of a small amount of Bi2GeO5 impurities (2θ=28.7°). Considering that the absorption band of Bi2GeO5 is located at ~350nm, trace impurities do not affect the subsequent analysis of the present invention.
[0047] The present invention first studies the optical properties of bismuth germanate. Under 272nm excitation, Bi4Ge3O 12 It exhibits broadband emission with a peak at 467nm. The emission peak originates from Bi 3+ of 3 P1→ 1 S0 transition. Figure 2a in the figure is the emission spectrum change of bismuth germanate (Example 1) before and after 12 hours of ultraviolet irradiation. After 12 hours of ultraviolet irradiation, the emission spectrum integral area of the bismuth germanate curve is reduced to 83% of the original. Figure 2 As shown in b, the integrated area of the XEL curve after ultraviolet irradiation is reduced to 84% of the original area. Irradiation can cause the luminescence intensity of bismuth germanate (Example 1) to decrease, which is not conducive to stability during use.
[0048] Figure 3 The photoluminescence emission spectrum of the cerium-doped bismuth germanate ceramic prepared in Example 4 before and after irradiation and the emission spectrum excited by X-rays, after ultraviolet irradiation, the emission spectrum integral area of the cerium-doped bismuth germanate ceramic powder becomes 106% of that before irradiation, and the emission spectrum integral area of the X-ray excited emission spectrum becomes 97% of the original. In contrast, doping with cerium can improve the ability of bismuth germanate to resist radiation damage.
[0049] In order to gain a deeper understanding of the electron capture and decapture behaviors involved in the irradiation process, high-resolution XPS measurements of Ce on the unirradiated and irradiated cerium-doped bismuth germanate ceramic samples prepared in Example 4 were performed. Figure 4 The valence distribution of Ce in a. 3+ and Ce 4+ Valence states coexist, mainly Ce 4+ Mainly, among which Ce 4+ 76% 3+ It accounts for 24% (x = 0.03). Irradiation will cause changes in the valence distribution. XPS after irradiation can see Ce 3+ Increase( Figure 4 b) Ce ions can effectively suppress X-ray radiation in Bi4Ge3O by changing valence. 12 The formation of color centers caused by 12 radiation resistance.
[0050] Figure 5 Bi 4-x Ge3O 12 :xCe (Examples 1, 2, 3, 4, 5, 6) Photoluminescence emission spectra of ceramic powder (excitation wavelength: λ ex=272nm) and the corresponding normalized integrated area. With the increase of cerium doping concentration, the photoluminescence intensity first decreases and then increases, reaching the lowest emission intensity at x=0.03. When the doping concentration is 0.005, 0.01, 0.03, 0.05, and 0.1, the integrated intensity of the emission spectrum is 66%, 68%, 29%, 55%, and 77% of that of undoped bismuth germanate. This shows that doping with cerium can have the effects of reducing luminescence intensity and improving radiation resistance. In addition, the increase in cerium concentration causes the emission peak to red-shift, which can reduce spectral self-absorption to a certain extent.
[0051] Figure 6 Shows Bi 4-x Ge3O 12 :xCe (Examples 1, 2, 3, 4, 5, 6) Excitation spectra of ceramic powders (monitoring wavelength: λ em =467nm), the peak of the excitation spectrum is located at 272nm, indicating that cerium doping does not introduce a new excitation peak.
[0052] Figure 7 The X-ray excitation emission diagrams of Examples 1, 3, 4, and 5 are given, which also illustrate that cerium doping can reduce the fluorescence output of bismuth germanate materials.
[0053] Figure 8 The decay curve of undoped bismuth germanate follows a single exponential equation with an average decay time of 328 ns, further verifying that the broadband emission is attributed to Bi 3+ electronic transition.
[0054] Bismuth germanate doped with cerium has a relatively short lifetime, which is crucial for fast scintillator response from an application point of view. In general, the fluorescence decay curve can detect the energy transfer process between dopants in the phosphor. Fig. 9 It was observed that the fluorescence lifetime became shorter after doping with Ce in Example 4 (the average decay time was 268 ns), which indicated that energy transfer occurred between the host and the cerium dopant.
[0055] Finally, it is necessary to explain here that the above embodiments are only used to further explain the technical solution of the present invention in detail and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above contents of the present invention all fall within the scope of protection of the present invention.
Claims
1. A cerium-doped bismuth germanate scintillating ceramic material, characterized in that: The chemical formula of the cerium-doped bismuth germanate scintillating ceramic material is Bi 4-x Ge3O 12 :xCe, where 0<x≤0.
1.
2. The cerium-doped bismuth germanate scintillating ceramic material according to claim 1, characterized in that: The Ce element is Ce 3+ and Ce 4+ The form of doping is in the Bi position; among which Ce 4+ Ce accounts for 70-80% of the total Ce element. 3+ The proportion of Ce is 20-30% of the total Ce element, and the sum of the two is 100%; when x = 0.03, Ce 4+ 76% 3+ Accounting for 24%.
3. The cerium-doped bismuth germanate scintillating ceramic material according to claim 1, characterized in that: x=0.01~0.05。 4. The cerium-doped bismuth germanate scintillating ceramic material according to any one of claims 1 to 3, characterized in that: The cerium-doped bismuth germanate scintillation ceramic material is in the form of ceramic powder or ceramic block.
5. The cerium-doped bismuth germanate scintillating ceramic material according to claim 4, characterized in that: The particle size of the ceramic powder is 50nm-50μm.
6. A method for preparing bismuth cerium germanate scintillating ceramic material, characterized in that: The chemical formula of the cerium-doped bismuth germanate scintillating ceramic material is Bi 4-x Ge3O 12 :xCe, where 0<x≤0.1; The cerium-doped bismuth germanate scintillation ceramic material is in the form of ceramic powder, and the preparation method comprises: (1) According to the chemical formula of cerium-doped bismuth germanate scintillating ceramic material Bi4Ge3O 12 :xCe weigh Bi source, Ge source and Ce source and mix them to obtain a mixed powder; (2) Sintering the mixed powder at 800-900° C. for 1-10 hours to obtain the cerium-doped bismuth germanate scintillating ceramic material.
7. The preparation method according to claim 6, characterized in that: The Bi source is Bi2O3; the Ge source is GeO2; and the Ce source is at least one of CeO2, Ce2O3, CeF3, and Ce(NO3)3.
8. The preparation method according to claim 6 or 7, characterized in that: The sintering atmosphere is air atmosphere, oxygen atmosphere or reducing atmosphere; the reducing atmosphere is a mixture of inert atmosphere and hydrogen, and the hydrogen content does not exceed 10 vol%.
9. A method for preparing bismuth cerium germanate scintillating ceramic material, characterized in that: The chemical formula of the cerium-doped bismuth germanate scintillating ceramic material is Bi 4-x Ge3O 12 :xCe, where 0<x≤0.1; The cerium-doped bismuth germanate scintillation ceramic material is in the form of a ceramic block, and the preparation method comprises: (1) According to the chemical formula of cerium-doped bismuth germanate scintillating ceramic material Bi4Ge3O 12 :xCe weigh Bi source, Ge source and Ce source and mix them to obtain a mixed powder; (2) pressing the mixed powder into a shape to obtain a ceramic green body; (3) The ceramic green body is subjected to hot pressing or hot isostatic pressing to obtain the cerium-doped bismuth germanate scintillating ceramic material.
10. The preparation method according to claim 9, characterized in that: The Bi source is Bi2O3; the Ge source is GeO2; and the Ce source is selected from at least one of CeO2, Ce2O3, CeF3, and Ce(NO3)3.
11. The preparation method according to claim 9 or 10, characterized in that: The parameters of the hot pressing sintering include: pressure of 0.03-5 GPa, sintering temperature of 500-900° C., and sintering time of 1-20 hours; The parameters of the hot isostatic pressing sintering include: a pressure of 0.03 to 5 GPa, a sintering temperature of 500 to 900° C., and a sintering time of 1 to 20 hours.
12. An application of the cerium-doped bismuth germanate scintillating ceramic material according to any one of claims 1 to 5 in the field of radiation detection, characterized in that: The radiation detection field includes high energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection and industrial detection.
Citation Information
Patent Citations
Ce3+ mixed lanthanum yttrium oxide transparent flickering ceramic material and preparation method thereof
CN101148356A
Method for preparing Ce3+ mixed lutecium oxide base transparent flickering ceramic material
CN101215171A
Method for obtaining a polycrystalline bismuth orthogermanate
RU2659268C1