Cerium-doped bismuth germanate single crystal scintillator and preparation method and application thereof
By doping cerium elements in bismuth germanate scintillator to form Bi4Ge3O12:Ce single crystal, the problems of BGO scintillator light output saturation, radiation damage and long attenuation time are solved, and higher radiation resistance and better Short attenuation time, suitable for high-energy physics and large scientific installations.
Patent Information
- Application Number
- CN202310590409.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
Bismuth germanate (BGO) scintillators have problems with light output saturation, radiation damage and long attenuation times in high-energy physics and large scientific devices, limiting their application in high-counting rate radiation detection and strong radiation environments.
Bi4Ge3O12:Ce single crystal scintillator is formed by doping cerium element (Ce). The doping amount of Ce element is between 0.005% and 0.7% by weight. Ce ions exist in the form of Ce3+ and Ce4+ in BGO, occupying the crystals of Bi3+ ions. The lattice position suppresses the formation of color center caused by radiation, reduces light output and improves radiation resistance, while shortens the attenuation time.
It significantly reduces the light output of BGO scintillator, improves radiation resistance, shortens its attenuation time, improves scintillation characteristics, and meets the characteristics of high-energy physics and large scientific devices to material light output, radiation resistance and time response. Higher requirements.
Smart Images

Figure CN119020863A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cerium-doped bismuth germanate single crystal scintillator for improving the scintillation performance of bismuth germanate, a preparation method and application thereof, and belongs to the field of scintillators for radiation detection. Background Art
[0002] Scintillators are a type of functional material that can absorb the energy of high-energy particles or radiation and convert it into ultraviolet-visible or near-infrared photons, which are then converted into electrical signals through photodetectors such as photomultipliers and silicon photomultipliers (SiPMs), thereby accurately detecting and identifying the type, quantity, energy, direction and position of incident high-energy particles or rays. Scintillator-based scintillation detectors have been widely used in high-energy physics, medical imaging, security inspection, resource exploration, environmental monitoring and industrial testing.
[0003] Doping is a reliable means to improve and improve the deficiencies of existing scintillating materials. With the differentiated needs of radiation detection, while researching and developing new scintillators with better performance, people have been trying to improve the scintillation performance of existing materials with large-scale manufacturing capabilities through doping, such as calcium-cerium co-doping to shorten the decay time of lutetium silicate crystals and enhance their light output (MASpurrier et al., Effects of Ca2+). 2+ Co-Doping on the Scintillation Properties of LSO: Ce, IEEE Trans. Nucl. Sci., 55 (2008): 1178-1182), yttrium doping suppresses the slow scintillation component in barium fluoride scintillation crystals, which has a light output 4-5 times that of the fast scintillation component (J. Chen et al., Slow Scintillation Suppression in Yttrium Doped BaF2 Crystals, IEEE Trans. Nucl. Sci. 65 (2018): 2147-2151), fluorine doping improves the light output of lead tungstate scintillation crystals, and yttrium doping improves its light transmittance and photoresponse uniformity (Wang Shaohua, Macroscopic defects in lead tungstate crystals and their doping effects, doctoral dissertation of Shanghai Institute of Ceramics, Chinese Academy of Sciences, 1999).
[0004] Bismuth germanate (Bi4Ge3O 12 , BGO) crystal is an inorganic scintillator with excellent comprehensive performance and high density (7.13g / cm 3 ), large effective atomic number (Z eff, 74), with outstanding advantages such as strong radiation blocking ability, high detection efficiency, moderate energy resolution, large intrinsic peak / comon ratio, good uniformity, no luminescent self-absorption, no afterglow, stable physical and chemical properties and good machinability, it has extensive and important applications in high-energy physics, astrophysics, nuclear physics, nuclear medical imaging, geological exploration, oil well logging and industrial detection. Since the 1980s, the crystal has been mass-produced, and with the deepening of research and development, there have been continuous breakthroughs in size and performance. It is still one of the most important and largest-scale inorganic scintillators. The Circular Electron Positron Collider (CEPC) and the Future Circular Collider (FCC) are large scientific facilities at the forefront of intensity, and the beam intensity is significantly higher than that of the existing Large Hadron Collider (LHC) and other devices, which puts higher requirements on the hardness and time response characteristics of scintillating crystals.
[0005] Silicon photomultiplier (SiPM) is a new type of highly sensitive semiconductor photodetector device, which consists of an array of multiple pixels connected in parallel in Geiger mode. Each pixel is composed of an avalanche photodiode and a quenching resistor in series. SiPM has the characteristics of high quantum efficiency, high gain, good signal-to-noise ratio, fast time response, low operating voltage, magnetic field insensitivity and compact structure. It has become the preferred scintillation photodetector device for devices such as CEPC and FCC, and is also the preferred choice for light readout of various scintillation detectors. Due to the large number of scintillation photons generated by GeV-TeV high-energy particles, when all pixels detect photons at the same time, the output signal of SiPM will be saturated, that is, there are no more pixels available to detect other incident photons, which will directly affect the dynamic range and accuracy of the electric energy device. Although the light output of the crystal can be reduced by attenuation plates, its stability and reliability in strong radiation environments cannot be guaranteed. Therefore, it is urgent to reduce the light output of BGO crystals to better meet the urgent application needs of large scientific facilities such as CEPC and FCC.
[0006] In addition, after being exposed to a certain dose of high-energy particles, rays or ultraviolet radiation, the BGO crystal will fade due to coloring, which will affect the crystal light output and light response uniformity. This is called "irradiation damage". How to reduce the radiation damage effect has always been one of the important research and development directions of BGO crystals. In addition, BGO crystals have a long decay time of ~0.3μs, which limits their application in high-count rate radiation detection such as high-energy physics and resource exploration. How to shorten their decay time has also received continuous attention. Summary of the invention
[0007] To this end, the object of the present invention is to provide a cerium-doped bismuth germanate single crystal scintillator, which reduces the light output of the BGO scintillator, improves its radiation resistance and shortens its decay time, and a preparation method and application thereof.
[0008] In one aspect, the present invention provides a cerium-doped bismuth germanate single crystal scintillator, wherein the cerium-doped bismuth germanate single crystal scintillator has a chemical formula of Bi4Ge3O 12 :Ce, wherein the doping amount of Ce element does not exceed 0.7wt%. Preferably, the Ce element is Ce 3+ and Ce 4+ Two ionic forms exist.
[0009] In the present disclosure, after cerium doping BGO, Ce 3+ and Ce 4+ Two ion forms exist in BGO scintillator, due to and The ionic radius is much larger than The ionic radius, The ionic radius is slightly larger than that of Ce 3+ and Ce 4+ According to the general principle that the doped ions must have ionic radii similar to those of the substituted ions in the matrix lattice, after Ce ion doping, it will occupy the Bi 3+ ions in the lattice. Moreover, the irradiation change of Ce ions can inhibit the radiation in Bi4Ge3O 12 The formation of color centers caused by 12 In addition, the present invention reduces the light output of BGO by Ce doping, which not only inhibits radiation damage but also shortens its decay time, which has important research significance and practical value. The emission peak of the cerium-doped bismuth germanate single crystal scintillator in this patent does not move, thus avoiding the impact of the detection efficiency caused by the movement of the emission peak.
[0010] Preferably, the doping amount of Ce element is 0.005wt% to 0.5wt%, preferably the doping amount of Ce element is 0.01wt% to 0.4wt%, and more preferably the doping amount of Ce element is 0.04wt% to 0.2wt%.
[0011] Preferably, the size of the cerium-doped bismuth germanate single crystal scintillator reaches the centimeter level in at least one dimension of length, width and height. Preferably, length×width×height is at least 1 cm×1 cm×1 cm.
[0012] On the other hand, the present invention provides a method for preparing a cerium-doped bismuth germanate single crystal scintillator, comprising: (1) According to the chemical composition Bi4Ge3O 12 :xCeWeigh Bi2O3 powder, GeO2 powder and Ce source and mix them to obtain a mixed powder; (2) The obtained mixed powder is directly loaded into a crucible or loaded into a crucible after a melting reaction, and grown by a crucible descent method, a pulling method, a kyberyzing method, a heat exchange method or a micro-pull-down method to obtain the cerium-doped bismuth germanate single crystal scintillator.
[0013] Preferably, the purity of the Bi2O3 powder is ≥99.9%; The purity of the GeO2 powder is ≥99.9%; The Ce source is selected from at least one of CeO2, Ce2O3 and Ce salt.
[0014] Furthermore, preferably, the Ce salt is selected from at least one of CeF3 and Ce(NO3)3.
[0015] Preferably, the temperature of the melting reaction is 900-1200° C., and the insulation time is 2-10 hours.
[0016] Preferably, the parameters of the crucible descent method include: a growth temperature of 900 to 1300° C.; and a descent rate of 0.2 to 1 mm / h.
[0017] Preferably, the parameters of the pulling method include: growth temperature of 900-1300° C.; rotation speed of 3-20 r / min; and pulling rate of 0.2-3 mm / h.
[0018] Preferably, the parameters of the pyrolysis method include: a growth temperature of 900 to 1300° C.; and a growth rate of 0.1 to 3 mm / h.
[0019] Preferably, the parameters of the heat exchange method include: growth temperature of 900-1300° C., constant temperature time of 1-24 hours; and cooling rate of 1-10° C. / h.
[0020] Preferably, the parameters of the micro-pull-down method include: a growth temperature of 1000-1300° C., and a crucible descending speed of 1-10 mm / h.
[0021] On the other hand, the present invention provides an application of a cerium-doped bismuth germanate single crystal scintillator in the field of radiation detection, which includes high-energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection and industrial detection. In practical applications, the cerium-doped bismuth germanate single crystal scintillator can be coupled with one of SiPM or PMT or CCD or CMOS detectors to form a small detection module, and the modules can be assembled into a two-dimensional or three-dimensional detection array according to actual application requirements; based on this, high-energy rays or particles interact with the detection array module and are recorded.
[0022] Beneficial effects of the present invention: The present invention can reduce the light output of BGO scintillator by doping with cerium, improve its radiation resistance, and shorten its decay time, which can significantly improve the scintillation characteristics of BGO. The cerium-doped bismuth germanate (BGO:Ce) single crystal scintillator obtained in the present invention can be used in radiation detection fields such as high-energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection, and industrial detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The actual pictures of pure BGO single crystal and BGO:Ce single crystal grown by the crucible descent method; Figure 2 is the UV-visible optical transmittance of pure BGO single crystal and BGO:Ce single crystal; Figure 3 Gamma-ray pulse height spectra of pure BGO single crystal and BGO:Ce single crystal; Figure 4 The normalized light output of pure BGO single crystal and BGO:Ce single crystal varies with irradiation time; Figure 5 Gamma-ray pulse time spectra of pure BGO single crystal and BGO:Ce single crystal. DETAILED DESCRIPTION
[0024] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0025] In the present disclosure, the chemical formula of the cerium-doped bismuth germanate single crystal scintillator is Bi4Ge3O 12 :Ce, wherein the doping amount of Ce element does not exceed 0.7wt% (for example, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, etc.). Preferably, the doping amount of Ce element is 0.005wt% to 0.5wt%, and more preferably the doping amount of Ce element is 0.04 to 0.2wt%. If the doping amount of Ce element is too high, the grown Bi4Ge3O 12 :Ce single crystal will produce more defects.
[0026] The following is an exemplary description of a method for preparing a cerium-doped bismuth germanate single crystal scintillator.
[0027] Bi2O3 and GeO2 are used as raw materials, and one or more Ce oxides or Ce salts such as CeO2, Ce2O3, CeF3, Ce(NO3)3, etc., containing cerium, are used as dopants. The raw materials are weighed according to the weight determined by the doping amount of the Ce element and then mixed to obtain a mixed powder.
[0028] The mixed powder is directly loaded into a single crystal growth crucible or loaded into a single crystal growth crucible after a melting reaction, and grown by using methods including but not limited to a crucible descent method, a Czochralski method, a kyvo method, a heat exchange method or a micro-pull-down method to obtain the cerium-doped bismuth germanate single crystal scintillator.
[0029] The invention reduces the light output of the crystal within an appropriate range by adjusting the doping amount of the cerium element, thereby improving the radiation resistance service capability of the crystal and increasing the time response rate of the crystal.
[0030] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0031] Example 1 Bi2O3 and GeO2 are used as raw materials, and CeO2 is used as a dopant, and the weight of the added amount is 0.01wt% (Bi2O3: 373.98g, GeO2: 125.97g, CeO2: 0.05g, i.e., mCeO2 / (mBi2O3+mGeO2+mCeO2)=0.01wt%), and then mixed to obtain a mixed powder; The obtained mixed powder is placed in a platinum crucible for single crystal growth, and the single crystal is grown by the crucible descent method to obtain a cerium-doped bismuth germanate single crystal scintillator. The parameters of the crucible descent method are as follows: first, the mixed powder is placed in a crystal growth furnace and heated at a constant temperature of 1300°C for 10 hours until the raw materials are completely melted. The crucible descent rate is 0.6mm / h, so that the melt slowly crystallizes from bottom to top. After the crystallization is completed, the temperature is cooled to room temperature at a cooling rate of 20°C / h to obtain a centimeter-level cerium-doped bismuth germanate single crystal scintillator.
[0032] Example 2 In this embodiment 2, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the amount of CeO2 added is 0.02wt%, the growth temperature is 1200℃, and the growth rate is 0.5mm / h.
[0033] Example 3 In this embodiment 3, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the amount of CeO2 added is 0.05wt%, the growth temperature is 1100°C, and the growth rate is 0.4mm / h.
[0034] Example 4 In this embodiment 4, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the amount of CeO2 added is 0.1wt%, the growth temperature is 1100°C, and the growth rate is 0.4mm / h.
[0035] Example 5 In this embodiment 5, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the dopant is CeF3, the addition amount is 0.2wt%, the growth method is the pulling method, the rotation speed is 10r / min, and the pulling rate is 1.0mm / h.
[0036] Example 6 In this embodiment 6, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 5, except that the amount of CeO2 added is 0.5wt%, the growth method is the kyvo method, the growth temperature is 1000°C, and the growth rate is 1mm / h.
[0037] Example 7 In this embodiment 7, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, with the following differences: the dopant is Ce(NO3)3, the addition amount is 0.1wt%, the growth method is heat exchange method, the growth temperature is 1100℃, the constant temperature time is 20 hours, and the cooling rate is 5℃ / h.
[0038] Example 8 In this embodiment 8, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the dopant is CeO2, the addition amount is 0.5wt%, and the growth rate is 0.4mm / h.
[0039] Example 9 In this embodiment 9, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the dopants are Ce(NO3)3 (50%) and CeO2 (50%), the added amount is 0.1wt%; the growth rate is 0.4mm / h.
[0040] Example 10 In this embodiment 10, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, with the following differences: the dopants are Ce(NO3)3 (50%), CeO2 (25%) and CeF3 (25%), the added amount is 0.1wt%, the growth method is micro-pull-down method, the growth temperature is 1100℃, and the crucible descent speed is 5mm / h.
[0041] Embodiment 11 In this embodiment 11, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.01wt% and the growth rate is 0.4mm / h.
[0042] Example 12 In this embodiment 12, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.02wt% and the growth rate is 0.4mm / h.
[0043] Embodiment 13 In this embodiment 13, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.2wt% and the growth rate is 0.4mm / h.
[0044] Embodiment 14 In this embodiment 14, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.3wt% and the growth rate is 0.4mm / h.
[0045] Embodiment 15 In this embodiment 15, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.4wt% and the growth rate is 0.4mm / h.
[0046] Example 16 In this embodiment 16, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.5wt% and the growth rate is 0.4mm / h.
[0047] Comparative Example 1 In this comparative example 1, Bi4Ge3O 12 The preparation process of the single crystal is similar to that of Example 1, except that the amount of CeO2 added is 0 wt%.
[0048] Table 1 is the Bi4Ge3O 12 : Preparation parameters of Ce single crystal:
[0049] Table 2 shows some Bi4Ge3O prepared by the present invention. 12 :Ce single crystal performance parameters:
[0050] Figure 1 The following are photos of pure BGO (left) and BGO:Ce (middle, Ce doping amount is 0.04wt%; right, Ce doping amount is 0.08wt%) single crystals grown by the crucible descent method. Figure 2 UV-Vis optical transmittance of pure BGO and BGO:Ce single crystals, from Figure 1 and 2 It can be seen that after doping with Ce element, single crystals with high optical quality can be grown. The crystal changes from colorless and transparent to light yellow, and the absorption edge shows a significant red shift.
[0051] Figure 3 The gamma-ray pulse height spectra of pure BGO and BGO:Ce single crystals are given. Figure 3 It can be seen that after doping with Ce element, the channel address characterizing the crystal light output is reduced from 703 of pure crystal to 201 (Ce element doping amount is 0.04wt%), 160 (Ce element doping amount is 0.08wt%) and 204 (Ce element doping amount is 0.16wt%) of Ce-doped crystal.
[0052] In order to study the radiation resistance of crystals, UVB ultraviolet light was used to irradiate pure BGO and BGO:Ce single crystals. Figure 4 The curves of the normalized light output of pure BGO and BGO:Ce single crystals changing with ultraviolet irradiation time are given in the figure. It can be seen from the figure that the radiation resistance of the crystal is significantly improved after the Ce element is doped, and the saturated irradiation light output is reduced from 25% of the pure BGO crystal to 5%. After saturated irradiation, the light output of the crystal can be maintained at about 95% before irradiation. That is, with the increase of the Ce element doping concentration, the radiation resistance of the crystal is first significantly enhanced, and then slightly reduced, but still maintained above 95%. This is mainly because the doping of Ce elements can significantly improve the radiation resistance of the crystal, but with the further increase of the doping concentration, it will lead to an increase in macroscopic defects in the crystal, making it difficult to further improve the radiation resistance. Therefore, the most preferred Ce element doping amount is 0.04wt% to 0.2wt%.
[0053] In order to determine the changing trend of the time response characteristics of BGO crystal after irradiation, the present invention uses an oscilloscope method to obtain the anode signal pulses of pure BGO and BGO:Ce single crystals under gamma ray excitation, thereby roughly obtaining the gamma ray pulse time spectrum of pure BGO and BGO:Ce crystals. Figure 5It can be seen that the decay time of the BGO crystal after doping with Ce element is significantly shortened from 381ns (pure BGO crystal) to 253ns (Ce element doping amount is 0.08%), and the decay constant is shortened by 33.6%, which significantly improves the time response characteristics of the BGO crystal. This is mainly because the doping of Ce element changes the crystal field strength of the activator Bi ion in the crystal, changes the Bi ion, increases the probability of radiation or non-radiation transition, thereby shortening the decay time and making it have better time response performance.
[0054] In the present invention, the Ce-doped bismuth germanate scintillator has lower light output, stronger radiation resistance and shorter decay time compared to pure bismuth germanate scintillator, and can meet the higher requirements of high-energy physics and other applications on material light output, radiation resistance and time response characteristics.
[0055] Finally, it is necessary to explain here that the above embodiments are only used to further explain the technical solution of the present invention in detail and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above contents of the present invention all fall within the scope of protection of the present invention.
Claims
1. A cerium-doped bismuth germanate single crystal scintillator, It is characterized in that The cerium-doped bismuth germanate single crystal scintillator has a chemical formula of Bi 4 Ge 3 O 12 :Ce, wherein the doping amount of Ce element does not exceed 0.7wt%.
2. The cerium-doped bismuth germanate single crystal scintillator according to claim 1, It is characterized in that The Ce element is Ce 3+ and Ce 4+ Two ionic forms exist.
3. The cerium-doped bismuth germanate single crystal scintillator according to claim 1, It is characterized in that The doping amount of Ce element is 0.005wt% to 0.5wt%.
4. The cerium-doped bismuth germanate single crystal scintillator according to claim 3, It is characterized in that The doping amount of Ce element is 0.04wt% to 0.2wt%.
5. The cerium-doped bismuth germanate single crystal scintillator according to any one of claims 1 to 4, It is characterized in that The size of the cerium-doped bismuth germanate single crystal scintillator reaches the centimeter level in at least one dimension of length, width and height.
6. A method for preparing the cerium-doped bismuth germanate single crystal scintillator according to any one of claims 1 to 5, It is characterized in that include: (1) Weigh Bi according to mass percentage 2 O 3 Powder, GeO 2 powder and a Ce source are mixed to obtain a mixed powder; (2) The obtained mixed powder is directly loaded into a crucible or loaded into a crucible after a melting reaction, and grown by a crucible descent method, a pulling method, a temperature gradient method, a heat exchange method, a kyberyzing method or a micro-pull-down method to obtain the cerium-doped bismuth germanate single crystal scintillator.
7. The preparation method according to claim 6, It is characterized in that The Bi 2 O 3 The purity of powder is ≥99.9%; The GeO 2 The purity of powder is ≥99.9%; The Ce source is selected from CeO 2 、Ce 2 O 3 and at least one of Ce salts; wherein the Ce salt is selected from CeF 3 、Ce(NO 3 ) 3 At least one of .
8. The preparation method according to claim 6, It is characterized in that The temperature of the melting reaction is 900-1200° C., and the insulation time is 2-10 hours.
9. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the crucible descent method include: a growth temperature of 900 to 1300° C.; and a descent rate of 0.2 to 1 mm / h.
10. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the pulling method include: a growth temperature of 900 to 1300° C.; a rotation speed of 3 to 20 r / min; and a pulling rate of 0.2 to 3 mm / h.
11. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the pyrolysis method include: a growth temperature of 900 to 1300° C.; and a growth rate of 0.1 to 3 mm / h.
12. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the heat exchange method include: a growth temperature of 900 to 1300° C., a constant temperature time of 1 to 24 hours, and a cooling rate of 1 to 10° C. / h.
13. The preparation method according to any one of claims 6 to 8, It is characterized in that The growth temperature of the micro-pull-down method is 1000-1300° C., and the crucible descending speed is 1-10 mm / h.
14. Use of the cerium-doped bismuth germanate single crystal scintillator according to any one of claims 1 to 5 in the field of radiation detection, It is characterized in that The radiation detection field includes high energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection and industrial detection.