Polyvinyl alcohol film and optical film prepared from same
By regulating the swelling degree and storage modulus turning point temperature of the polyvinyl alcohol film in boric acid solution, the polarization decay and high-temperature edge and corner warping of the polyvinyl alcohol film are solved, and efficient polarization film performance and stability are achieved.
Patent Information
- Application Number
- CN202310658893.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2023-06-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-06-06
Smart Images

Figure CN119019737A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polyvinyl alcohol (PVA) product, in particular to a polyvinyl alcohol film and an optical film made therefrom, but not limited thereto. Background Art
[0002] Polyvinyl alcohol (PVA) film is a hydrophilic material obtained by coating and drying an aqueous solution containing polyvinyl alcohol polymer and a plasticizer. It has high transparency, mechanical strength, water solubility, good processability and other properties. It has been widely used in various optical films for packaging materials or electronic products, such as polarizing films.
[0003] The polarizing film obtained by processing the polyvinyl alcohol film through the polarization process (manufacturing process) has the characteristic of only allowing light in a specific direction to pass through, and can thereby control the brightness of the light passing through; based on this characteristic, the polarizing film is used in various displays, glasses and wearable devices, becoming an indispensable component. The so-called polarizing process generally includes steps such as swelling, stretching and dyeing; specifically, the polyvinyl alcohol film will be placed in a solution to perform the above steps, allowing the dye molecules to diffuse into the molecules in the polyvinyl alcohol film, and through stretching to obtain a relatively regular arrangement, so that the polarizing film can absorb the light component parallel to its arrangement direction and allow the light component in the perpendicular direction to pass through, thereby generating polarization characteristics.
[0004] The polarizing film should have suitable optical properties, such as high polarization and low polarization decay value. To this end, the prior art changes the structure of polyvinyl alcohol or adds functional groups to improve the optical properties. Prior art such as Taiwan Invention Patent Publication No. 202231448 provides a polarizing film with excellent polarization performance and small shrinkage stress. When manufacturing the polarizing film, the total necking rate (A), the necking rate in the stretching step (B), and the necking rate in the drying step (C) are controlled at the same time. By controlling the total necking rate (A), the reduction of polarization performance and yield can be suppressed. In addition, by appropriately controlling the necking rate (B) in the stretching step and the necking rate (C) in the drying step, a polarizing film with excellent polarization performance and small shrinkage stress can be manufactured.
[0005] In addition, the prior art, such as the polarizing film disclosed in Taiwan Invention Patent Publication No. 202212872, uses a dyed triacetyl cellulose film as a protective layer to inhibit the polarization degree of the polarizing film from decreasing under a high temperature and high humidity environment. Summary of the invention
[0006] In the prior art, when using polyvinyl alcohol film to prepare optical films, it is still common to find that the polarization degree seriously declines after long-term use. In this regard, the inventors have found that by adjusting the polyvinyl alcohol film, making it soaked in a specific concentration of boric acid solution, temperature and time, it has a specific range of surface swelling, and the storage modulus (E') in a specific temperature range has a specific range of turning point temperature; the polarizing film produced will have excellent polarization, and the problem of polarization degree decline of the optical film after long-term use can be improved.
[0007] Specifically, on one hand, the present invention provides a polyvinyl alcohol film, which comprises a polyvinyl alcohol resin with a degree of alkalinity of 95 mol% or more; wherein the surface swelling of the polyvinyl alcohol film obtained by immersing it in a 4wt% boric acid solution at 55°C for 1 minute is 17.0% to 38.0%, and the storage modulus (E') of the polyvinyl alcohol film in water in the range of 30°C to 55°C has a turning point temperature of 37 to 40°C.
[0008] In one or more embodiments, the polyvinyl alcohol film has a swelling degree of 17.5% to 35.0%, and the turning point temperature is 37.8 to 38.5°C.
[0009] In one or more embodiments, the polyvinyl alcohol film is immersed in a 4 wt % boric acid solution at 55° C. for 1 minute, and the swelling degree in the TD (Transverse Direction) direction is 9.0% to 18.0%, and the swelling degree in the MD (Machine Direction) direction is 7.5% to 18.0%.
[0010] In one or more embodiments, the TD swelling degree of the polyvinyl alcohol film is 9.0% to 16.50%, and the MD swelling degree is 8.0% to 16.0%.
[0011] In one or more embodiments, the absolute value of the difference between the swelling degree in the TD direction and the swelling degree in the MD direction of the polyvinyl alcohol film is less than or equal to 5%.
[0012] In one or more embodiments, the ratio of the TD swelling degree to the MD swelling degree of the polyvinyl alcohol film is 0.9 to 1.7.
[0013] In one or more embodiments, the ratio of the TD swelling degree to the MD swelling degree of the polyvinyl alcohol film is 0.95 to 1.60.
[0014] In one or more embodiments, the average degree of polymerization of the polyvinyl alcohol film is 1500 to 3500.
[0015] In one or more embodiments, the average degree of polymerization of the polyvinyl alcohol film is 2000 to 3500.
[0016] In one or more embodiments, the polyvinyl alcohol film has a thickness of 30 to 75 μm.
[0017] Another aspect of the present invention provides an optical film, which is made from the polyvinyl alcohol film.
[0018] In one or more embodiments, the optical film is a polarizing film.
[0019] In one or more embodiments, the polarization degree of the polarizing film is greater than or equal to 99.99%.
[0020] In one or more embodiments, the polarization film is heat-treated at 80° C. for 500 hours, and the polarization decay value thereof is less than or equal to 0.01%.
[0021] In one or more embodiments, the polarizing film is heat treated at 80° C. for 500 hours, and its surface shrinkage is less than or equal to 2%.
[0022] In one or more embodiments, the polarizing film is heat treated at 80° C. for 500 hours, and its TD direction shrinkage rate and MD direction shrinkage rate are both less than or equal to 1%.
[0023] The polyvinyl alcohol film of the present invention can be used for various purposes, and is particularly suitable for preparing optical films, such as polarizing films. The polarizing films prepared using the polyvinyl alcohol film obtained by the technical content of the present invention have excellent polarization and can improve the decay of polarization after long-term use.
[0024] In addition, the inventors have also found that when the polyvinyl alcohol film of the present invention is controlled to have a specific range of swelling when immersed in a boric acid solution of a specific concentration, temperature and time, an optical film with improved shrinkage can be made; further, when the polyvinyl alcohol film has a specific range of TD swelling and a specific range of MD swelling, the optical film made therefrom has improved shrinkage in the corresponding directions. Thus, the present invention can avoid the situation where the corners of the optical film are warped due to long-term use in a high-temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a curve diagram showing the change of storage modulus (E') of a polyvinyl alcohol film in water as a function of temperature according to an embodiment of the present invention;
[0026] Figures 2 to 4 FIG. 4 is a schematic diagram of a sample preparation method for analyzing the turning point temperature of a polyvinyl alcohol film according to an embodiment of the present invention. DETAILED DESCRIPTION
[0027] In order to make the description of the present invention more detailed and complete, the following is an illustrative description of the implementation and specific embodiments of the present invention, but this is not the only form of implementing or using the specific embodiments of the present invention. In this specification and the attached patent scope, unless the context otherwise states, "a", "an" and "the" may also be interpreted as plural.
[0028] Although the numerical ranges and parameters used to define the present invention are approximate values, the relevant numerical values in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations caused by individual testing methods. Here, the term "about" means that the actual value falls within the acceptable standard error of the mean value, which is determined by those with ordinary knowledge in the field to which the present invention belongs.
[0029] [Polyvinyl alcohol film]
[0030] On one hand, the present invention provides a polyvinyl alcohol film, which comprises a polyvinyl alcohol resin with a basicity of 95 mol% or more; wherein the polyvinyl alcohol film is immersed in a 4wt% boric acid solution at 55°C for 1 minute, and the surface swelling degree obtained is 17.0% to 38.0%, and the storage modulus (E') of the polyvinyl alcohol film in water at 30°C to 55°C has a turning point temperature of 37 to 40°C. According to some embodiments, the thickness of the polyvinyl alcohol film of the present invention is 30 to 75μm. Specifically, the range of any two of the following values, for example: 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, the aforementioned values are only illustrative and not restrictive.
[0031] The "swelling degree" mentioned in this article includes the "surface swelling", "TD direction (Transverse Direction) swelling (hereinafter referred to as TD direction swelling)" and "MD direction (Machine Direction) swelling (hereinafter referred to as MD direction swelling)" of the polyvinyl alcohol film. The "surface swelling obtained by immersing the polyvinyl alcohol film in 4wt% boric acid solution at 55°C for 1 minute (hereinafter referred to as surface swelling)" mentioned in this article is obtained by calculating the area change of the polyvinyl alcohol film after immersing the polyvinyl alcohol film in 4wt% boric acid solution at 55°C for 1 minute.
[0032] The polyvinyl alcohol film has a crystalline region and an amorphous region. When the polyvinyl alcohol film is immersed in a boric acid solution, the aqueous solution containing boric acid will enter the amorphous region in the film and dissolve part of the crystals; the boric acid in the solution will further cross-link and bond with the molecules. The inventors found that the numerical range of the surface swelling degree is related to the polarization degree of the optical film produced subsequently, the polarization degree decay situation and the shrinkage rate of the optical film. It is speculated that when more crystals are dissolved, the number of bonds with boric acid increases, making the intermolecular structure more stable. The possible reason is that when the crystals are partially dissolved, the chain segments at the dissolved position are relatively orderly in arrangement, and can move freely and change the distance between the chain segments, which can produce more positions suitable for boric acid bonding; while the chain segments that are amorphous themselves have fewer positions that can bond with boric acid because of their uncertain spacing and disorderly arrangement. Thus, when the swelling degree of the polyvinyl alcohol film is too low, it means that there are fewer crystals dissolved, and the number and area of the chain segments that can be cross-linked with boric acid are also small, resulting in a less stable intermolecular structure, which is easily changed by heat, and then leads to the decline of the polarization degree of the subsequent optical film, and is easy to shrink and deform the polarizing film. On the other hand, when the swelling degree is too high, it means that too many crystals are dissolved in the polyvinyl alcohol film, which leads to insufficient crystallization of the polyvinyl alcohol film, which reduces the physical strength of the film and makes it easy to break.
[0033] Therefore, in order to make the polyvinyl alcohol film have both a stable intermolecular structure and good physical strength, the surface swelling degree needs to be controlled within a specific range; specifically, the surface swelling degree of the polyvinyl alcohol film of the present invention after being immersed in a 4wt% boric acid solution at 55°C for 1 minute is 17.0% to 38.0%, such as within the range of any two of the following values, for example: 17.0%, 17.5%, 18.0%, 18.5%, 19.0%, 19.5%, 20.0%, 20.5%, 21.0%, 21.5%, 22.0%, 22.5%, 23.0%, 23.5%, 24. %, 35.0%, 35.5%, 36.0%, 36.5%, 37.0%, 37.5%, or 38.0%; preferably, the surface swelling degree of the polyvinyl alcohol film is 17.5 to 35.0% or 35%.
[0034] The "modulus" described in this article is a physical property used to analyze the relationship between stress and strain in material mechanics, which is the ratio of stress to strain. If the stress applied to the material is a positive force, the modulus obtained is represented by E. The "storage modulus (E')" is the stored internal energy converted from the material absorbing the applied energy, which is usually used to recover deformation and maintain the original appearance of the material. It is related to the elastic characteristics of the material. It can also reflect the rigidity of the material. From the molecular point of view, the higher the storage modulus (E'), the stronger the intermolecular force.
[0035] The "storage modulus (E') in water in the range of 30°C to 55°C has a turning point temperature (hereinafter referred to as the E' turning point temperature)" described in this article is obtained by immersing the polyvinyl alcohol film in water and measuring the change in the storage modulus (E') of the polyvinyl alcohol film in a temperature increase mode. After a large amount of water is absorbed by the membrane, the molecular chains of polyvinyl alcohol swell and separate, resulting in a decrease in the entanglement between the molecular chains. At this time, the response of the storage modulus (E') is more affected by the crystallization in the membrane; therefore, the storage modulus (E') analysis of polyvinyl alcohol immersed in water can be used to evaluate the change in crystallinity in the membrane at different temperatures. Furthermore, the storage modulus (E') curve of the polyvinyl alcohol film in water analyzed as a function of temperature has the following characteristics: Figure 1 The characteristic of the change curve between 30℃ and 55℃ is that there are two different slopes, and the intersection of the tangents of the two slopes is the E' turning point, and the corresponding temperature is the E' turning point temperature (such as Figure 1 (where the arrow points).
[0036] The inventors have found that the physical meaning of the E' turning point temperature includes that it is the temperature at which the crystals in the polyvinyl alcohol film begin to dissolve in large quantities; if the E' turning point temperature is higher, it indicates that the average crystal particles in the film are larger, and thus a large amount of crystal dissolution occurs only at relatively high temperatures. Without being limited by a particular theory, it is speculated that when the crystal particle size is controlled within a suitable range, the polyvinyl alcohol film will have the most suitable number and area of crystal residues for crosslinking with boric acid, so that the polarization degree of an optical film (such as a polarizing film) made from the polyvinyl alcohol film will not easily decline under high temperature and long-term use.
[0037] Therefore, in order to obtain the above-mentioned effect, the E' turning point temperature needs to be controlled within a specific range; specifically, the storage modulus (E') of the polyvinyl alcohol film of the present invention in water in the range of 30°C to 55°C (the temperature range of the first stretching in the polarizing film manufacturing process) has a turning point temperature of 37 to 40°C, such as but not limited to: 37°C, 37.1°C, 37.3°C, 37.5°C, 37.7°C, 37.9°C, 38°C, 38.1°C, 38.3 ℃, 38.5℃, 38.7℃, 38.9℃, 39℃, 39.1℃, 39.3℃, 39.5℃, 39.7℃, 39.9℃ or 40℃; preferably, the E' turning point temperature of the polyvinyl alcohol film is 37.8 to 38.5℃, such as in the range of any two of the following values, for example: 37.8℃, 37.9℃, 38.0℃, 38.1℃, 38.2℃, 38.3℃, 38.4℃ or 38.5℃. It should be noted that when the measuring temperature is greater than 55℃, the physical properties of the polyvinyl alcohol film may change drastically due to the complete disappearance of crystallization. Therefore, when analyzing the turning point temperature, the set analysis temperature range should avoid exceeding 55℃.
[0038] In addition, regarding the aforementioned method of measuring the E' inflection point temperature, since the polyethylene film will absorb water (even moisture in the air) and affect its crystal state, before measuring the E' inflection point temperature of the polyethylene film, the moisture content of each polyethylene film to be measured can be adjusted to be consistent through pre-treatment, so that the state to be measured of each polyethylene film is consistent. The moisture content can usually be adjusted to about 8wt% to 9wt%, but this is not limited to this in this article.
[0039] The "basicity" described herein is a measured value obtained according to the JIS K 6726 (1994) standard test method. In one or more embodiments, the basicity of the polyvinyl alcohol-based resin is 95 mol% or more, for example: 95 mol% or more, 95.5 mol% or more, 96 mol% or more, 96.5 mol% or more, 97 mol% or more, 97.5 mol% or more, 98 mol% or more, 98.5 mol% or more, 99 mol% or more or 99.5 mol% or more. According to one embodiment of the present invention, the basicity of the polyvinyl alcohol-based resin of the present invention is greater than 99.90 mol%, for example, greater than 99.90 mol%, greater than 99.92 mol%, greater than 99.94 mol%, greater than 99.96 mol% or greater than 99.98 mol%; preferably, the basicity of the polyvinyl alcohol-based resin is greater than 99.95 mol%, for example, greater than 99.95 mol%, greater than 99.97 mol% or greater than 99.99 mol%; more preferably, the basicity of the polyvinyl alcohol-based resin is greater than 99.97 mol%, for example, greater than 99.97 mol%, greater than 99.98 mol% or greater than 99.99 mol%.
[0040] The "swelling in the TD direction (hereinafter referred to as the TD swelling) and the swelling in the MD direction (hereinafter referred to as the MD swelling) obtained by immersing the polyvinyl alcohol film in a 4wt% boric acid solution at 55°C for 1 minute" described in this article are obtained by respectively calculating the length changes of the polyvinyl alcohol film along the TD direction and along the MD direction after the polyvinyl alcohol film is immersed in a 4wt% boric acid solution at 55°C for 1 minute. Among them, the TD direction is also called the transverse direction, and the MD direction is also called the mechanical direction. Without being limited by a specific theory, when the swelling in the TD direction and the swelling in the MD direction of the polyvinyl alcohol film are respectively controlled within a specific range, the shrinkage rates of the optical film made subsequently in the TD and MD directions can be reduced respectively, so that the optical film attached to the display device can avoid the corner warping of the optical film under high temperature and long-term use.
[0041] Therefore, in order to obtain the above-mentioned effects, the TD direction swelling degree of the polyvinyl alcohol film of the present invention is 9.0% to 18.0%, such as within the range of any two of the following values, for example: 9.0%, 9.5%, 10.0%, 10.5%, 11.0%, 11.5%, 12.0%, 12.5%, 13.0%, 13.5%, 14.0%, 14.5%, 15.0%, 15.5%, 16.0%, 16.5%, 17.0%, 17.5% or 18.0%; more preferably, the TD direction swelling degree of the polyvinyl alcohol film is 9.0% to 16.5%; and, the swelling degree of the polyvinyl alcohol film in the MD direction is 7.5% to 16.0%, such as in the range of any two of the following values, for example: 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, 10.5%, 11.0%, 11.5%, 12.0%, 12.5%, 13.0%, 13.5%, 14.0%, 14.5%, 15.0%, 15.5% or 16.0%; more preferably, the swelling degree of the polyvinyl alcohol film in the MD direction is 8.0% to 16.0%.
[0042] In one or more embodiments, the absolute value of the difference between the swelling degree in the TD direction and the swelling degree in the MD direction of the polyvinyl alcohol film is less than or equal to 5%, for example: less than or equal to 5%, less than or equal to 4.5%, less than or equal to 4%, less than or equal to 3.5%, less than or equal to 3%, less than or equal to 2.5%, less than or equal to 2%, less than or equal to 1.5%, less than or equal to 1% or less than or equal to 0.5%.
[0043] In one or more embodiments, the ratio of the TD direction swelling to the MD direction swelling of the polyvinyl alcohol film is 0.95 to 1.60, such as within the range of any two of the following values, for example: 0.95, 1.00, 1.05, 1.10, 1.15, 1.20, 1.25, 1.30, 1.35, 1.40, 1.45, 1.50, 1.55 or 1.60.
[0044] Without being limited by a specific theory, when the absolute value or ratio of the difference between the swelling degree in the TD direction and the swelling degree in the MD direction is too large, the display subsequently manufactured including the polyvinyl alcohol film may experience peeling between the polarizing film and the protective layer or between the polarizing film and the glass, thereby causing the display to deteriorate.
[0045] The "average degree of polymerization" described herein is measured according to the JIS K 6726 (1994) standard test method. In one or more embodiments, the average degree of polymerization of the polyvinyl alcohol film is 1500 to 3500, such as in the range of any two of the following values, for example: 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400 or 3500; preferably, the average degree of polymerization of the polyvinyl alcohol film is 2000 to 3500.
[0046] Without being limited by a specific theory, the inventors have found that the above-mentioned surface swelling, E' turning point temperature, TD swelling and MD swelling can be controlled by adjusting the average degree of polymerization of the resin raw material of the polyvinyl alcohol film; in addition, it can also be controlled by adjusting the dissolution temperature and time of the raw materials in the manufacturing method, the total drying time at a temperature greater than 50°C and the molecular orientation of the polyvinyl alcohol polymer in the polyvinyl alcohol film, but is not limited to this.
[0047] [Method for producing polyvinyl alcohol film]
[0048] The method for manufacturing the polyvinyl alcohol film of the present invention generally comprises the following steps: (a) a dissolution process: heating a polyvinyl alcohol resin to dissolve it, and adjusting the concentration of the polyvinyl alcohol resin to form a polyvinyl alcohol casting solution; (b) a casting process: casting the polyvinyl alcohol casting solution onto a casting drum, and obtaining a polyvinyl alcohol preformed film after peeling off from the casting drum; (c) a hot roller process: obtaining a polyvinyl alcohol film semi-finished product after the polyvinyl alcohol preformed film is contacted with a plurality of hot rollers; (d) an oven process: placing the polyvinyl alcohol film semi-finished product in an oven to dry, thereby obtaining a polyvinyl alcohol film finished product; and (e) a temperature and humidity control process: placing the polyvinyl alcohol film finished product in a temperature and humidity control box, adjusting the temperature and humidity to obtain a polyvinyl alcohol film; wherein, in the above-mentioned hot roller and oven processes, the total drying time at a temperature greater than 50° C. is controlled to be 10 to 20 minutes.
[0049] [Dissolution process]
[0050] According to some embodiments, the dissolution process mainly involves raising the temperature of the polyvinyl alcohol resin, solvent, plasticizer, etc. to 130 to 165°C while stirring, dissolving for 1 to 5 hours, adjusting the resin to an appropriate concentration, and then obtaining a polyvinyl alcohol casting solution. The appropriate concentration of the resin is about 20wt% to 50wt%, for example: 20wt%, 30wt%, 40wt% or 50wt%; if the resin concentration is too low, the subsequent film drying load becomes high; conversely, if the resin concentration is too high, the viscosity is too high, which will make film making difficult.
[0051] In one or more embodiments, the polyvinyl alcohol resin used in the aforementioned dissolution process is obtained by polymerizing vinyl ester resin monomers to form a polyvinyl ester resin with an average degree of polymerization of 1500 to 3500, and then undergoing a saponification reaction to obtain a polyvinyl alcohol resin with a basicity greater than 95 mol%. It is believed that the average degree of polymerization can affect the solubility and stretching of polyvinyl alcohol molecules in water, thereby affecting the crystal particles and crystallinity of the finished polyvinyl alcohol film. The greater the degree of polymerization, the larger the crystal particles of the finished polyvinyl alcohol film and the higher the crystallinity; however, too high a degree of polymerization will make the crystal particles too large, thereby affecting the E' turning point temperature; in addition, too low a degree of polymerization will make the E' turning point too low, and the mechanical strength of the film will also be too low.
[0052] Among them, the vinyl ester resin monomer can be vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate or vinyl octanoate, or a combination thereof, which is not limited in the present invention. Preferably, vinyl acetate is used. In addition, the aforementioned vinyl ester resin monomer can also be modified by copolymerization by adding olefin compounds or acrylate derivatives. Among them, the olefin compound can be ethylene, propylene or butene, etc., which is not limited in the present invention; the addition amount of the olefin compound can be but not limited to 2mol% to 4mol%, such as 2mol%, 2.5mol%, 3mol%, 3.5mol% or 4mol%, etc. The acrylate derivative can be acrylic acid, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate or n-butyl acrylate, etc., which is not limited in the present invention.
[0053] In one or more embodiments, the solvent used in the aforementioned dissolution process can be used as long as it can dissolve the polyvinyl alcohol resin, so it is not limited in the present invention. As the solvent, for example, but not limited to: water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylenediamine, diethylenetriamine, etc., the above solvents can be used alone or in combination of two or more. Considering the environment and economic aspects, water is preferably used as the solvent in the present invention.
[0054] In one or more embodiments, the "plasticizer" described herein may be, but is not limited to, glycerol, ethylene glycol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol or trimethylolpropane, or a combination of any of the aforementioned plasticizers; glycerol is preferred in the present invention. In one or more embodiments, the amount of the plasticizer added relative to the weight of the polyvinyl alcohol resin is 5wt% to 15wt%, specifically, for example but not limited to 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% and 15wt%, and in a preferred embodiment, the amount of the plasticizer added relative to the weight of the polyvinyl alcohol resin is 10wt%.
[0055] In addition to the above-mentioned plasticizers, other additives may be further added in the dissolution process as needed, including but not limited to surfactants (surfactants), etc.; the surfactants include but are not limited to cationic, anionic or non-ionic surfactants, and specifically may be but are not limited to: carboxylate type such as potassium laurate, sulfate ester type such as sodium laureth sulfate, sulfonate type such as dodecylbenzenesulfonate, alkylphenyl ether type such as polyoxyethylene octylphenyl ether, alcohol phenyl ether type such as polyethylene glycol monooctylphenyl ether, alkyl ester type such as polyoxyethylene laurate, alkylamine type such as polyoxyethylene laurylamine ether, alkylamide type such as polyoxyethylene lauramide, polypropylene glycol ether type such as polyoxyethylene polyoxypropylene ether, lauric acid diethanolamide, oleyl diethanolamide, allylphenyl ether type such as polyoxyalkylene allylphenyl ether, or sodium lauryl alcohol polyoxyethylene ether sulfate, etc.
[0056] In one or more embodiments, the temperature for dissolving the polyvinyl alcohol resin aqueous solution is preferably 130 to 165°C, such as the range of any two of the following values, specifically for example: 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C or 165°C. It is believed that the dissolution temperature affects the dissolution of the polyvinyl alcohol resin and the dispersion of the additive. When the dissolution temperature is higher, the dissolution of the polyvinyl alcohol resin and the dispersion of the additive are better, so that the crystal particles of the formed polyvinyl alcohol film are smaller and the crystallinity is lower; however, when the dissolution temperature is too high, it may cause the formed polyvinyl alcohol film to partially yellow. On the contrary, without being limited by a specific theory, when the dissolution temperature is too low, the dissolution of the polyvinyl alcohol resin and the dispersion of the additive are not good, and the crystal particles of the formed polyvinyl alcohol film are larger, which leads to the E' turning point temperature of the polyvinyl alcohol film being too high.
[0057] In one or more embodiments, the time for dissolving the polyvinyl alcohol resin aqueous solution is preferably 1 to 5 hours, such as the range of any two of the following values, specifically for example: 1 hour, 2 hours, 3 hours, 4 hours or 5 hours. It is believed that the dissolution time affects the dissolution of the polyvinyl alcohol resin and the dispersion of the additive. When the dissolution time is longer, the dissolution of the polyvinyl alcohol resin and the dispersion effect of the additive are better, thereby making the crystalline particles of the polyvinyl alcohol film smaller and the crystallinity lower. On the contrary, without being limited by a specific theory, when the dissolution time is too short, the dissolution of the polyvinyl alcohol resin and the dispersion effect of the additive are not good, and the crystalline particles of the formed polyvinyl alcohol film are larger, which leads to the excessively high E' turning point temperature of the polyvinyl alcohol film.
[0058] [Casting process]
[0059] According to some embodiments, the casting process mainly involves conveying the polyvinyl alcohol casting solution to a twin-screw extruder, and then mixing and defoaming the solution again in the extruder (for example, but not limited to defoaming using a twin-screw extruder), and then discharging the solution from a T-slit die lip and casting the solution onto a rotating high-temperature casting drum (or casting roller), an endless belt, or the like as a support to form a film on the casting drum, thereby obtaining a polyvinyl alcohol primary formed film. In one or more embodiments, during the casting process, the conveying temperature of the polyvinyl alcohol casting solution during conveying is preferably controlled to be at least 90° C. or above, such as but not limited to: 90° C., 91° C., 92° C., 93° C., 94° C., 95° C., 96° C., 97° C., 98° C. or 99° C.; in addition, the polyvinyl alcohol casting solution after being mixed and defoamed again by the extruder must also be controlled to be at least 90° C. or above, such as but not limited to: 90° C., 91° C., 92° C., 93° C., 94° C., 95° C., 96° C., 97° C. or 98° C.
[0060] In one or more embodiments, when the polyvinyl alcohol casting solution is cast onto the rotating high-temperature casting drum, the temperature of the casting drum is preferably 85 to 95° C., and the polyvinyl alcohol stays on the casting drum for preferably 0.6 to 1.2 minutes.
[0061] [Hot Roller Process]
[0062] According to some embodiments, the hot roller process mainly involves drying the upper and lower surfaces of the polyvinyl alcohol preformed film peeled off from the casting drum by contacting a plurality of hot rollers to further obtain a polyvinyl alcohol film semi-finished product. The temperature of the plurality of hot rollers (e.g., 13 to 19 hot rollers) gradually decreases from high to low, and the starting hot roller is the hottest one among all the hot rollers (e.g., but not limited to, 90 to 99°C, specifically, for example, but not limited to, 90, 91, 92, 93, 94, 95, 96, 97, 98 or 99°C), and the temperature of the final hot roller is the coldest one among all the hot rollers (e.g., but not limited to, 25 to 40°C, specifically, for example, but not limited to, 25, 30, 35 or 40°C).
[0063] [Oven process]
[0064] According to some embodiments, the oven process mainly uses an oven to dry the upper and lower surfaces of the polyvinyl alcohol film semi-finished product after peeling off the hot roller (for example, but not limited to drying with hot air and infrared light), thereby obtaining a polyvinyl alcohol film finished product. In one or more embodiments, the oven is preferably a floating oven, and its temperature is controlled between 100 and 120°C, for example: 100°C, 105°C, 110°C, 115°C or 120°C; preferably 110°C.
[0065] Among them, in one or more embodiments, in the above-mentioned hot roller process and oven process, the total drying time at a temperature greater than 50°C is 10 to 20 minutes, specifically, for example: 10 minutes, 15 minutes or 20 minutes. It is believed that the total drying time at a temperature greater than 50°C will affect the surface swelling, TD swelling, MD swelling and E' turning point temperature of the polyvinyl alcohol film. Not limited by a specific theory, it is speculated that since the glass transition temperature of the finished polyvinyl alcohol film is 40 to 50°C when the moisture content is 2wt%, the polymer chain can move freely in a small range when the drying temperature is greater than 50°C. Therefore, when the total drying time is longer, the crystal particles are larger and the crystallinity is higher; conversely, when the total drying time is shorter, the crystal particles are smaller and the crystallinity is lower, which in turn affects the swelling and E' turning point temperature of the polyvinyl alcohol film.
[0066] [Temperature and humidity control process]
[0067] According to an embodiment of the present invention, after the above-mentioned process is completed, the finished polyvinyl alcohol film can be placed in a temperature and humidity control box to adjust the temperature and humidity.
[0068] In one or more embodiments, the temperature of the temperature and humidity control box is between 35 and 45°C, specifically in the range between any two of the following values, for example: 35°C, 40°C or 45°C, preferably 45°C. In one or more embodiments, the relative humidity of the temperature and humidity control box is preferably between 40% and 60%, specifically in the range between any two of the following values, for example: 40%, 45%, 50%, 55% or 60%, preferably 50%. In one or more embodiments, the polyvinyl alcohol film is preferably placed in the temperature and humidity control box for 20 to 40 minutes, for example: 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes. In one or more embodiments, for example, the polyvinyl alcohol film is placed in a temperature and humidity control box with a temperature of 45°C and a relative humidity of 50% for 30 minutes.
[0069] In addition, according to an embodiment of the present invention, during the oven process, the film can be further clamped with a clamp on both sides, and additional tension in the TD direction can be applied to maintain the size of the film in the TD direction to adjust the molecular orientation of the film. Since the polyvinyl alcohol film is generally stretched in the MD direction, the polyvinyl alcohol polymer is easily aligned along the MD direction; therefore, after additional force is applied to the film in the TD direction, the orientation of the polyvinyl alcohol polymer can be balanced, thereby reducing the difference in swelling between the two directions.
[0070] [Optical film]
[0071] Another object of the present invention is to provide an optical film, which is made from the aforementioned polyvinyl alcohol film. The "optical film" mentioned herein can be a polarizing film, a phase difference film, a viewing angle enhancement film or a brightness enhancement film, etc., especially a polarizing film.
[0072] The "polarization degree" described herein is measured according to the standard method of JIS Z 8722. In one or more embodiments, the polarization degree of the polarizing film of the present invention is greater than or equal to 99.99%; for example, greater than or equal to 99.990%, greater than or equal to 99.992%, greater than or equal to 99.994%, greater than or equal to 99.996%, and greater than or equal to 99.998%.
[0073] In one or more embodiments, the polarizing film is heat treated at 80° C. for 500 hours, and its polarization decay value is less than or equal to 0.01%; for example, less than or equal to 0.010%, less than or equal to 0.009%, less than or equal to 0.008%, less than or equal to 0.007%, less than or equal to 0.006% or less than or equal to 0.005%.
[0074] In one or more embodiments, the polarizing film is heat treated at 80° C. for 500 hours, and its surface shrinkage is less than or equal to 2%; for example, less than or equal to 2%, less than or equal to 1.9%, less than or equal to 1.8%, less than or equal to 1.7%, less than or equal to 1.6%, less than or equal to 1.5%, or less than or equal to 1.4%.
[0075] In one or more embodiments, the polarizing film is heat treated at 80° C. for 500 hours, and its TD direction shrinkage rate and MD direction shrinkage rate are both less than or equal to 1%; for example, both are less than or equal to 1%, both are less than or equal to 0.95%, both are less than or equal to 0.90%, both are less than or equal to 0.85%, both are less than or equal to 0.80%, and both are less than or equal to 0.75%.
[0076] [Method for producing optical film]
[0077] According to some embodiments, the "method for manufacturing an optical film" described in this case refers to a method for manufacturing a polarizing film, and further refers to manufacturing a polyvinyl alcohol film into a polarizing film. The method for manufacturing a polarizing film includes a dyeing step for adsorbing iodine ions, a boric acid treatment step, and a water washing step; a uniaxial stretching step can be implemented in the boric acid treatment step or in a stage before the step. Preferably, a swelling step for swelling the polyvinyl alcohol film with water can be provided before the dyeing step. In addition, a final drying step is usually provided after the water washing step.
[0078] In the swelling step, the polyvinyl alcohol film is immersed in a treatment bath (e.g., pure water) at a temperature of 30 to 55° C. to wash the film surface and swell it. The swelling treatment time is usually 5 to 300 seconds, preferably 20 to 240 seconds. According to some embodiments, a plurality of guide rollers are arranged in the swelling tank containing the treatment bath to transport the polyvinyl alcohol film. Subsequently, the polyvinyl alcohol film is stretched in the MD direction to 1.05 to 2.5 times of the original length, and then the dyeing step is performed.
[0079] In the dyeing step, the polyvinyl alcohol film after the above-mentioned swelling step is immersed in a dyeing tank containing a dyeing bath. The conditions of the dyeing treatment can be determined based on the range within which the iodine is adsorbed on the polyvinyl alcohol film without causing adverse conditions such as extreme dissolution and devitrification of the film. The dyeing bath in the dyeing step is, for example, an aqueous solution containing iodine and potassium iodide, and the concentration of iodine in the dyeing bath is preferably 0.01wt% to 0.5wt%, and the concentration of potassium iodide is preferably 0.01wt% to 10wt%; a specific example may be, but is not limited to, an aqueous solution of iodine with a concentration of 0.037wt% and potassium iodide with a concentration of 1.85wt%. In addition, other iodides such as zinc iodide can also be used instead of potassium iodide, or other iodides can be used in addition to potassium iodide. The temperature of the dyeing bath is usually 20 to 40°C, for example 20°C, 30°C or 40°C, and the time of the dyeing treatment (dyeing time) is usually 10 to 600 seconds, preferably 30 to 200 seconds. Next, the polyvinyl alcohol film is stretched along a machine direction to 2 to 4 times of its original length, and then subjected to a boric acid treatment and a stretching step.
[0080] In the boric acid treatment and extension step, the iodine-dyed polyvinyl alcohol film is treated with an aqueous solution containing boric acid to make it cross-linked, and the adsorbed iodine is fixed in the resin. This step is usually carried out by immersing the polyvinyl alcohol film after the dyeing step in a fixing tank containing a treatment bath containing boric acid. The boric acid treatment bath preferably contains iodide in addition to boric acid. The iodide used can be potassium iodide or zinc iodide, for example, an aqueous solution containing boric acid and potassium iodide at a concentration of 5.5wt%. In addition, compounds other than iodide can also coexist in the boric acid treatment bath, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, sodium sulfite, potassium sulfate, sodium sulfate, etc. The boric acid treatment and extension step is usually carried out at 50 to 70°C, preferably at 55°C; and the treatment time is usually 10 to 600 seconds, preferably 20 to 300 seconds, and more preferably 20 to 100 seconds. Next, the polyvinyl alcohol film is stretched along the mechanical direction to more than 3 times of its original length before proceeding to subsequent steps; the upper limit of the stretching ratio is not particularly limited, but is preferably less than 8 times, for example, stretched to include but not limited to 3.3 times or more, such as 3.3 to 8.0 times, more preferably 3.5 to 6.0 times, and particularly preferably 4.0 to 5.5 times.
[0081] After the polyvinyl alcohol film has gone through the above steps and the subsequent washing and drying steps, a polarizing film is formed. In the washing and drying steps, the iodine solution and boric acid remaining on the film surface are washed with water or an aqueous solution containing iodide, for example but not limited to washing with a potassium iodide aqueous solution with a concentration of 5.5wt%. Then, after a drying step, for example but not limited to drying in an oven at a temperature of 60°C for 5 minutes, a polarizing film is formed. Furthermore, a protective layer can be formed on at least one side of the polarizing film to make a polarizing film product (or polarizer). In detail, the protective layer is preferably a component having functions such as preventing surface wear of the polarizing film, and comprises a transparent resin. According to different embodiments, the protective layer can be provided on only one side of the polarizing film, but is preferably formed on both sides of the polarizing film. The protective layer can be a protective film of a transparent resin material; the transparent resin can be an acrylic resin such as methyl methacrylate resin, an olefin resin, a polyvinyl chloride resin, a cellulose resin, a styrene resin, an acrylonitrile-butadiene-styrene copolymer resin, an acrylonitrile-styrene copolymer resin, a polyvinyl acetate resin, a polyvinylidene chloride resin, a polyamide resin, a polyacetal resin, a polycarbonate resin, a modified polyphenylene ether resin, a polyester resin (polybutylene terephthalate resin, polyethylene terephthalate resin, etc.), a polysulfone resin, a polyethersulfone resin, a polyarylate resin, a polyamide-imide resin, a polyimide resin, an epoxy resin, an oxetane resin, etc.; preferably, a cellulose resin is used, for example, triacetate cellulose (TAC).
[0082] Example
[0083] Hereinafter, the present invention will be further described with detailed description and specific examples. However, it should be understood that these specific examples are only used to help the present invention to be more easily understood and are not used to limit the scope of the present invention.
[0084] 1. Polyvinyl alcohol film preparation
[0085] Here, the present invention provides a non-limiting method for preparing polyvinyl alcohol films. According to a method similar to the method disclosed below, non-limiting example polyvinyl alcohol films (Examples 1 to 12) and comparative example polyvinyl alcohol films (Comparative Examples 1 to 5) were prepared.
[0086] The following are the main steps common to the present embodiment and the comparative example in manufacturing the polyvinyl alcohol film, and the following Table 1 will show in detail the differences in one or more process parameters between the present embodiment and the comparative example:
[0087] [Dissolution process]: Add 1800 kg of polyvinyl alcohol resin with an average degree of polymerization of 1500 to 3500 (as shown in Table 1) and a basicity of 99.95 mol%, 4000 kg of water, and 180 kg of plasticizer glycerol into a dissolution tank, and raise the dissolution temperature to 130 to 165°C (as shown in Table 1) while stirring, and control the dissolution time to 1 to 5 hours (as shown in Table 1); after the dissolution is uniform, add water to adjust the resin concentration to 30wt% to obtain a polyvinyl alcohol casting solution. Among them, the polyvinyl alcohol resin used in the embodiment and the comparative example is a polyvinyl alcohol resin polymerized from vinyl acetate and unmodified (i.e., does not contain other comonomers); in addition, the specific average degree of polymerization, dissolution temperature, and dissolution time of the polyvinyl alcohol resin are shown in Table 1.
[0088] [Casting process]: The polyvinyl alcohol casting solution is transported to a double-screw extruder, mixed and defoamed again by the extruder, and the casting solution temperature is controlled to 98°C. The casting solution is then extruded from a T-slit die lip and cast onto a rotating high-temperature casting drum for drying and forming a primary film.
[0089] [Hot Roller Process]: After the polyvinyl alcohol preformed film is peeled off from the casting drum, 13 hot rollers are used to contact the upper and lower surfaces of the dry film. The first hot roller has the highest temperature of all the hot rollers, which is 95°C. The temperature of the subsequent hot rollers gradually decreases from high to low, and the temperature of the 13th hot roller drops to 30°C.
[0090] [Oven process]: Use a floating oven for drying, and use hot air and infrared light to dry the upper and lower sides of the film to produce a polyvinyl alcohol film product. In different examples, when using a floating oven for drying, clamps can be used to clamp the two sides of the film to apply tension in the TD direction to maintain the size of the film in the TD direction.
[0091] Among them, in the above casting, hot roller and oven processes, the total drying time at a temperature greater than 50° C. is controlled (the specific time is shown in Table 1).
[0092] [Temperature and humidity control process]: Subsequently, the finished polyvinyl alcohol film is placed in a temperature and humidity control box at a temperature of 45° C. and a relative humidity of 50% for 30 minutes to obtain a polyvinyl alcohol film.
[0093] Table 1
[0094] 2. Polarizing film preparation
[0095] Here, the present invention provides a non-limiting method for preparing an optical film from a polyvinyl alcohol film, specifically a non-limiting method for preparing a polarizing film. According to the method disclosed below, the non-limiting example polyvinyl alcohol films (Examples 1 to 12) and the comparative example polyvinyl alcohol films (Comparative Examples 1 to 5) are prepared into corresponding polarizing films.
[0096] The following are the main steps for preparing polarizing films in the embodiments of the present invention and the comparative examples: after unwinding the polyvinyl alcohol film, let it enter the swelling tank filled with 30°C pure water to wash and swell the film surface; after the polyvinyl alcohol film is stretched to 1.2 times of the original length in the mechanical direction, it then enters the dyeing tank controlled at 30°C and containing an aqueous solution of 0.037wt% iodine and 1.85wt% potassium iodide to dye, and the polyvinyl alcohol film is extended to 3.4 times of the original length in the mechanical direction; after dyeing, it enters the extension tank controlled at 55°C and containing an aqueous solution of 5.5wt% boric acid and potassium iodide, and after the polyvinyl alcohol film is extended to 6 times of the original length in the mechanical direction, the iodine solution and boric acid remaining on the film surface are washed with an aqueous solution containing 5.5wt% potassium iodide. Then, it is dried in a 60°C oven for 5 minutes, and the upper and lower surfaces are laminated with triacetyl cellulose protective films and dried to form a polarizing film.
[0097] 3. Analytical methods
[0098] Here, the present invention provides analysis and testing methods for the polyvinyl alcohol films of Examples 1 to 12 and Comparative Examples 1 to 5.
[0099] Alkalinity The basicity determination method of the present invention is based on the JIS K 6726 (1994) standard method.
[0100] Average degree of polymerization The method for measuring the degree of polymerization in the present invention is based on the JIS K 6726 (1994) standard method.
[0101] Swelling 1. Test conditions: Cut the polyvinyl alcohol film into square samples of 10 cm in MD direction and 10 cm in TD direction. Clamp the edges of the sample to the glass with binder clips and immerse it in 55°C 4wt% boric acid solution for 1 minute to allow it to swell. After swelling is completed, take out the sample together with the glass, remove the binder clips, flatten the swollen sample, and measure the lengths in the MD and TD directions after swelling with a vernier ruler. 2. Calculation formula for swelling degree in each direction (MD direction and TD direction): 3. Calculation formula of surface swelling degree:
[0102] E' turning point temperature 1. Instrument and brand: TA Instruments DMA 850 2. Sample preparation method: Cut the polyvinyl alcohol film into strips with a length of 5 cm in the machine direction (MD) and 5 mm in the width direction (TD). Before loading the film, adjust the moisture content of the polyvinyl alcohol film to 8wt% to 9wt% to make the polyvinyl alcohol film uniform. Figure 2 , clamp one end of the polyvinyl alcohol film 2 with a dovetail clip 3 of about 1.11g, and insert the other end into the immersion stretching fixture 1, so that a part of the polyvinyl alcohol film 2 is placed between the fixed axis 1a and the lower fixed axis 1b, so that the lower end 3a of the dovetail clip 3 is 1cm away from the immersion stretching fixture 1 ( Figure 2 The distance a) shown in FIG. 1 is a distance between the upper end 2a of the polyvinyl alcohol film 2 and the upper end of the immersion stretching fixture 1, and a reserved space is provided; then, the upper fixing shaft 1a is locked to fix the polyvinyl alcohol film 2. Next, refer to Figure 3 , vertically place the entire immersion stretching fixture 1 together with the polyvinyl alcohol film 2 and dovetail clamp 3 held by it into a 100mL beaker 4 filled with pure water so that the liquid level of the beaker is located on the upper fixed axis, and control the temperature of the beaker 4 in a 30℃ constant temperature water tank (not shown in the figure) to allow the polyvinyl alcohol film 2 to swell under a load (the weight of the dovetail clamp 3) for 20 minutes. Finally, refer to Figure 4 , take out the immersion and stretching fixture 1 from the beaker 4 and keep it upright, use the weight of the dovetail clamp 3 to stretch the polyvinyl alcohol film 2, and after ensuring that the polyvinyl alcohol film 2 is centered, lock the lower fixed axis 1b of the immersion and stretching fixture 1, and then remove the excess polyvinyl alcohol film 2c (i.e. Figure 4 The grid-like part in the middle is cut off, and the sample is the polyvinyl alcohol film 2b that is swollen under load and clamped in the immersion and stretching fixture 1. 3. Test conditions: With the sample still fixed in the immersion and stretching fixture, select the oscillation heating mode, place the sample together with the immersion and stretching fixture holding it into an immersion tank filled with deionized water, set the frequency to 1Hz, the amplitude to 200μm, the holding pressure (force track) to 200%, and the temperature to be measured from 30℃ to 65℃. Before the analysis, the film is stretched with a static force of 0.15N before starting the analysis at a heating rate of 1℃ / min and plotting the storage modulus (E') versus temperature. The thermocouple sensing end is placed 5mm above the bottom of the tank. 4. Data processing: Change the coordinate axis of the storage modulus (E') to a linear coordinate axis, use the onset analysis built into the software included with the instrument, set the onset analysis temperature range to 30 to 45°C, and the software will automatically bring out the turning point temperature.
[0103] 4. Evaluation methods and results
[0104] Here, the present invention provides evaluation methods for polyvinyl alcohol films and polarizing films of Examples and Comparative Examples, and results corresponding to the above-mentioned analysis contents.
[0105] Polarization evaluation
[0106] Test conditions: Cut the polarizing film into two square samples of 4 cm in MD direction and 4 cm in TD direction. Overlap the two polarizing film samples in parallel in MD direction (i.e. flow direction). Use a spectrophotometer to measure the light transmittance (H) under the irradiation of light with a wavelength of 700 nm. 11 ); The two polarizing film samples are then overlapped in a form perpendicular to the MD direction, and the transmittance (H1) is measured under the irradiation of light with a wavelength of 700 nanometers, and the polarization degree is calculated by the following formula: Polarization degree (%) = [(H 11 -H1) / (H 11 +H1)] 1 / 2 .
[0107] Polarization decay value evaluation
[0108] Test conditions: The polarizing film was placed in an oven at 80°C for heat treatment for 500 hours, the polarization degree was remeasured, and the polarization degree decay value was calculated using the following formula: Polarization degree decay value (%) = |Polarization degree after heat treatment - original polarization degree|.
[0109] Furthermore, the surface swelling degree and E' turning point temperature of the polyvinyl alcohol films of Examples 1 to 12 of the present invention and Comparative Examples 1 to 5 are presented in Table 2 together with the polarization degree evaluation and polarization degree decay value evaluation of the corresponding polarizing films.
[0110] Table 2
[0111] According to Table 2, the surface swelling of the polyvinyl alcohol film samples of Examples 1 to 12 is measured in the range of 17.0% to 38.0% in the analysis of the surface swelling and the E' turning point temperature, and the E' turning point temperature is 37 to 40°C; the polarization degree of the polarizing films made from these polyvinyl alcohol films is greater than 99.99%, and the polarization degree decay value is less than or equal to 0.010%, thereby obtaining excellent polarization evaluation and polarization degree decay value evaluation. On the contrary, the surface swelling and the E' turning point temperature of the polyvinyl alcohol film samples of Comparative Examples 1 to 5 cannot fall within the above-mentioned specific ranges at the same time in the analysis of the surface swelling and the E' turning point temperature, and the polarization degree decay value of the polarizing films made from these polyvinyl alcohol films is greater than 0.010%, and it is impossible to obtain ideal results in the polarization evaluation and the polarization degree decay value evaluation at the same time. In view of this, only by controlling the surface swelling of the polyvinyl alcohol film obtained by immersing it in a 4wt% boric acid solution at 55°C for 1 minute to be 17.0 to 38.0%, and the storage modulus (E') of the polyvinyl alcohol film in water in the range of 30°C to 55°C having a turning point temperature of 37 to 40°C, can the polarizing film obtained thereby have good polarization while also improving the polarization decay situation.
[0112] Shrinkage evaluation 1. Test conditions: Cut the polarizing film into square samples with a size of 10 cm in MD direction and 10 cm in TD direction, place them in an 80°C oven for 500 hours, take them out and return them to room temperature, then use a vernier ruler to measure the lengths in the MD and TD directions, and use the following shrinkage formula to calculate the MD shrinkage, TD shrinkage and surface shrinkage. 2. Shrinkage formula in each direction (MD direction and TD direction): 3. Surface shrinkage formula:
[0113] Furthermore, the TD direction swelling, MD direction swelling, swelling difference and swelling ratio (TD / MD) of the polyvinyl alcohol films of Examples 1 to 12 of the present invention and Comparative Examples 1 to 5 are presented in Table 3 together with the surface shrinkage, TD direction shrinkage and MD direction shrinkage of the corresponding polarizing film.
[0114] Table 3 Note: * indicates easy-to-break film
[0115] According to Table 3, the surface swelling, TD direction swelling and MD direction swelling of the polyvinyl alcohol films of Examples 1 to 12 are in the range of 17.0% to 38.0%, 9.0% to 18.0% and 7.5% to 18.0% respectively, so the polarizing film obtained has the characteristics of surface shrinkage less than or equal to 2%, TD direction shrinkage less than or equal to 1%, and MD direction shrinkage less than or equal to 1%. Further observation shows that although the surface shrinkage, TD direction shrinkage and MD direction shrinkage of the polarizing film in Comparative Example 3 are all ideal, the evaluation results of the polarization degree and the polarization degree decay value are not good, so it still does not have the effect to be achieved in this case, and it is found in the experimental process that the polyvinyl alcohol film is prone to film breakage during the polarizing film manufacturing process. In summary, when the surface swelling of the polyvinyl alcohol film is controlled to be 17.0% to 38.0%, the swelling in the TD direction is 9.0% to 18.0%, and the swelling in the MD direction is 7.5% to 18.0%, the polarizing film produced therefrom can further have the characteristics of small shrinkage and not easy to deform after long-term use in a high-temperature environment.
[0116] Herein, all ranges provided are intended to include each specific range within a given range and combinations of sub-ranges between the given ranges. In addition, unless otherwise stated, all ranges provided herein include the endpoints of the ranges. Thus, ranges 1-5 specifically include 1, 2, 3, 4, and 5, as well as sub-ranges such as 2-5, 3-5, 2-3, 2-4, 1-4, etc.
[0117] All publications and patent applications cited in this specification are incorporated herein by reference, and each individual publication or patent application is specifically and individually indicated to be incorporated herein by reference for any and all purposes. In the event of any inconsistency between this document and any publication or patent application incorporated herein by reference, this document controls. Explanation of symbols 1 Immersion tensile fixture 1a Upper fixed shaft 1b Lower fixed shaft 2 Polyvinyl alcohol film 2a Top 2b Polyvinyl alcohol film swollen under load 2c Excess polyvinyl alcohol film 3 Dovetail clamp 3a Bottom 4 Beaker a Distance
Claims
1. A polyvinyl alcohol film comprising a polyvinyl alcohol resin having a basicity of 95 mol % or more; wherein: The surface swelling degree of the polyvinyl alcohol film after being immersed in a 4 wt % boric acid solution at 55° C. for 1 minute is 17.0% to 38.0%, and the storage modulus (E') of the polyvinyl alcohol film in water at 30° C. to 55° C. has a turning point temperature of 37 to 40° C.
2. The polyvinyl alcohol film according to claim 1, wherein The surface swelling degree is 17.5% to 35.0%, and the turning point temperature is 37.8 to 38.5°C.
3. The polyvinyl alcohol film according to claim 1, wherein The polyvinyl alcohol film is immersed in a 4 wt % boric acid solution at 55° C. for 1 minute, and the swelling degree in the TD (Transverse Direction) direction is 9.0% to 18.0%, and the swelling degree in the MD (Machine Direction) direction is 7.5% to 18.0%.
4. The polyvinyl alcohol film according to claim 3, wherein The TD direction swelling degree is 9.0% to 16.5%, and the MD direction swelling degree is 8.0% to 16.0%.
5. The polyvinyl alcohol film according to claim 3, wherein The absolute value of the difference between the swelling degree in the TD direction and the swelling degree in the MD direction is less than or equal to 5%. 6 . The polyvinyl alcohol film according to claim 3 , wherein the ratio of the swelling degree in the TD direction to the swelling degree in the MD direction is 0.9 to 1.
7. 7 . The polyvinyl alcohol film according to claim 5 , wherein the ratio of the swelling degree in the TD direction to the swelling degree in the MD direction is 0.95 to 1.
60.
8. The polyvinyl alcohol film according to any one of claims 1 to 7, wherein The average polymerization degree of the polyvinyl alcohol resin is 1500 to 3500.
9. The polyvinyl alcohol film according to claim 8, wherein The average polymerization degree of the polyvinyl alcohol resin is 2,000 to 3,500.
10. The polyvinyl alcohol film according to any one of claims 1 to 7, wherein The polyvinyl alcohol film has a thickness of 30 to 75 μm.
11. An optical film made from the polyvinyl alcohol film according to any one of claims 1 to 10.
12. The optical film according to claim 11, which is a polarizing film.
13. The optical film of claim 12, wherein the polarization degree of the polarizing film is greater than or equal to 99.99%.
14. The optical film according to claim 12, wherein the polarization degree decay value of the polarizing film is less than or equal to 0.01% after heat treatment at 80°C for 500 hours.
15. The optical film according to claim 12, wherein the polarizing film has a surface shrinkage of less than or equal to 2% after being heat-treated at 80°C for 500 hours.
16. The optical film of claim 12, wherein the shrinkage ratio in the TD direction and the shrinkage ratio in the MD direction of the polarizing film after heat treatment at 80°C for 500 hours are both less than or equal to 1%.
Citation Information
Patent Citations
Polarizing plate, method for producing same, and polarizing plate with retardation layer and image display device, each using said polarizing plate
TW202212872A
Method for producing polarizing film and polarizing film
TW202231448A
Recording material
JP1985245586A
Polyvinyl alcohol film, optical film containing same, and methods for producing the same
JP7228722B1
Poly(vinyl alcohol) film and production method for polarizing film
US20210041613A1