Copper lignosulfonate-polyphosphazene cross-linked modified MXene flame retardant and preparation method thereof

By cross-linking polymerization of lignin sulfonate and phosphazene on the surface of MXene nanosheets and chelating transition metal copper ions, copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant was prepared, and Ti3C2Tx was solved The problems of limited flame retardant performance and poor compatibility have achieved efficient flame retardant and smoke suppression effects on PLA composites.

CN119019761APending Publication Date: 2024-11-26XIANGTAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411116483.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

As a separate flame retardant, Ti3C2Tx has limited flame retardant properties and its hydrophilicity leads to poor compatibility with PLA matrix, resulting in limited applications in the field of flame retardant.

Method used

By cross-linking and polymerizing lignin sulfonate and phosphazene on the surface of MXene nanosheets and chelating transition metal copper ions, copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant was prepared to enhance its resistance Fuel and smoke suppression properties and improve compatibility with PLA matrix.

Benefits of technology

It significantly improves the flame retardant and smoke suppression properties of PLA composite materials, and at the same time improves the hydrophobic properties of the flame retardant, reduces the negative impact on the mechanical properties of the PLA matrix, and enhances its dispersion and compatibility in PLA.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019761A_ABST
    Figure CN119019761A_ABST
Patent Text Reader

Abstract

The invention discloses a copper lignosulfonate-polyphosphazene cross-linked modified MXene flame retardant and a preparation method thereof.The copper lignosulfonate-polyphosphazene cross-linked modified MXene flame retardant is successfully prepared through cross-linking polymerization of lignosulfonate and phosphazene on the surfaces of MXene nanosheets and chelating of transition metal copper ions, the flame retardance and smoke suppression performance is obviously improved, and the flame retardance and smoke suppression performance are improved. The hydrophobicity and the compatibility with the PLA matrix can be improved, and the flame retardance and smoke suppression performance of the PLA composite material are improved while the deterioration of the mechanical property of the PLA matrix due to the addition of the flame retardant is reduced as much as possible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of flame retardancy, and specifically relates to a copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant and a preparation method thereof. Background Art

[0002] Ti3C2T x First discovered by Barsoum in 2011, Ti3C2T has attracted the attention of many researchers as a new type of two-dimensional nanomaterial due to its metal-like conductivity, adjustable surface properties and good mechanical properties. Due to its unique layered structure and outstanding pressure resistance, Ti3C2T x It has shown great potential in the fields of energy storage, sensors, electromagnetic interference shielding and photocatalysis. Even in the absence of other surfactants or binders, Ti3C2T x It also has good hydrophilicity and hydrocolloid stability, so it can be used to produce products with various structures such as fibers, films and aerogels. x As a very promising functional nanofiller with great research value, it can be easily dispersed in polymer materials, so that various types of polymer nanocomposites can be prepared to enhance the conductivity, fire safety and mechanical properties of the composites.

[0003] It is generally believed that well-dispersed two-dimensional nanosheets can produce a "maze effect" when burning in a polymer matrix, which can extend the airflow path in the matrix and form dense carbon residues, thereby effectively preventing further combustion of the polymer material. x As a typical two-dimensional nanomaterial, it has the characteristics of high specific surface area, excellent structural stability and thermal stability, so it can build a tight and protective physical barrier at high temperature. x The particles tend to form higher crystallinity and still maintain a layered morphology, with excellent structural stability. It is also considered to be an ideal reinforcing filler in other two-dimensional materials besides graphene. x The transition metal compounds produced by combustion in the polymer matrix are believed to have good catalytic effects, which can effectively hinder smoke release and facilitate the formation of carbon layers. x Thanks to the abundant terminal groups on the surface, it is easier to modify and can be well combined with the polymer matrix to prepare high-performance composite materials. Compared with other two-dimensional materials, Ti3C2T xIt has unique advantages in terms of the variability of structure and chemical composition, and its performance can be "tailor-made" to meet the needs of many special applications. Therefore, as a new member of many flame retardant types, Ti3C2T x It has attracted the attention of many researchers in the past few years and has also been used to flame retard various polymer materials. x It also exhibits some inherent defects, such as its limited flame retardant performance as a single flame retardant, and Ti3C2T x The hydroxyl groups on the surface make it easy to agglomerate. x The hydrophilicity of PET leads to very poor compatibility with PLA matrix, which seriously hinders its application in flame retardant field. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant and a preparation method thereof. The copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant is successfully prepared by cross-linking polymerization of lignin sulfonate and phosphazene on the surface of MXene nanosheets and chelating transition metal copper ions. The flame retardant and smoke suppression performance of the PLA composite material are improved while the hydrophobicity and compatibility with the PLA matrix are improved. The flame retardant and smoke suppression performance of the PLA composite material are improved while the deterioration of the mechanical properties of the PLA matrix caused by the addition of the flame retardant is minimized.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A method for preparing a copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant comprises the following steps:

[0007] (1) ultrasonically dispersing MXene in deionized water to obtain a MXene dispersion; adding APTES (3-aminopropyltriethoxysilane) to the MXene dispersion, stirring and mixing, and obtaining silanized MXene after solid-liquid separation;

[0008] (2) The silanized MXene and sodium lignin sulfonate (SLS) are ultrasonically dispersed in acetonitrile to obtain a mixed slurry; hexachlorotripolyphosphazene (HCCP) is ultrasonically dispersed in acetonitrile to obtain a hexachlorotripolyphosphazene solution; the hexachlorotripolyphosphazene solution and triethylamine (TEA) are simultaneously added dropwise to the mixed slurry, heated and stirred for reaction, and the solid sample obtained after solid-liquid separation is ultrasonically dispersed in deionized water, and copper chloride solution is added dropwise thereto, and the mixture is fully stirred to obtain a copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant, which is recorded as MXene / CLS-PZS

[0009] Those skilled in the art know that MXene, as a typical two-dimensional nanomaterial, can form a compact carbon layer at high temperature and the transition metal compounds in MXene have a good catalytic effect, which can effectively inhibit the release of smoke and facilitate the formation of a carbon layer. However, MXene still has some defects, such as its limited flame retardant performance as a single flame retardant, and the hydroxyl and other functional groups on the surface of MXene make it easy to agglomerate. In addition, Ti3C2T x The hydrophilicity of the polymer leads to very poor compatibility with the PLA matrix.

[0010] In view of this, the present invention successfully prepares a lignin sulfonate copper-polyphosphazene cross-linked modified MXene flame retardant by cross-linking polymerization of lignin sulfonate and phosphazene on the surface of MXene nanosheets and chelating transition metal copper ions, wherein the SO2 gas generated by the lignin sulfonate at high temperature promotes the foaming and expansion of the carbon layer while providing sufficient carbon source for the carbon layer, and the rich N and P elements in the phosphazene play a flame retardant role in the gas phase and the condensed phase: during combustion, it plays a free radical capture effect while releasing N2 and NH3 to dilute the concentration of O2 and combustible gas; the transition metal Ti and Cu elements synergistically catalyze and promote the polymer to form a thicker and more uniform carbon layer, which combines with the generated transition metal oxide to form a stable and dense physical barrier, isolating mass transfer, heat transfer and smoke escape, greatly enhancing the flame retardant and smoke suppression efficiency of PLA, and the lignin sulfonate copper-polyphosphazene coating layer can significantly improve the hydrophobicity of the flame retardant, thereby helping to improve the compatibility between the flame retardant and the PLA matrix.

[0011] In summary, the present invention successfully prepared lignin sulfonate copper-polyphosphazene cross-linked modified MXene flame retardant by cross-linking polymerization of lignin sulfonate and phosphazene on the surface of MXene nanosheets and chelating transition metal copper ions. This not only significantly improved the flame retardant properties, but also improved the hydrophobic properties and its compatibility with the PLA matrix, while minimizing the deterioration of the mechanical properties of the PLA matrix caused by the addition of the flame retardant, while improving the flame retardancy and smoke suppression properties of the PLA composite material.

[0012] Preferably, in step (1), the concentration of the MXene dispersion is 0.2-0.5 g:100 ml.

[0013] Preferably, in step (1), the mass volume ratio of MXene and APTES is 1 g: 30-50 ml.

[0014] Preferably, in step (2), the amounts of silylated MXene, sodium lignin sulfonate, hexachlorotriphosphazene and triethylamine are 1 g: 0.1-0.3 g: 0.05-0.2 g: 10-30 ml.

[0015] Preferably, in step (2), the heating temperature is 30 to 50° C. and the reaction time is 8 to 24 hours.

[0016] The present invention also provides a copper sulfonate-polyphosphazene cross-linked modified MXene flame retardant prepared by the above preparation method.

[0017] The advantages of the present invention are:

[0018] (1) The present invention successfully prepares a lignin sulfonate copper-polyphosphazene cross-linked modified MXene flame retardant by cross-linking and polymerizing lignin sulfonate and phosphazene on the surface of MXene nanosheets and chelating transition metal copper ions. The SO2 gas generated by lignin sulfonate at high temperature promotes the foaming and expansion of the carbon layer while providing sufficient carbon source for the carbon layer. The rich N and P elements in phosphazene play a flame retardant role in both the gas phase and the condensed phase: during combustion, it plays a free radical capture effect while releasing N2 and NH3 to dilute the concentration of O2 and combustible gas; the transition metal Ti and Cu elements synergistically catalyze and promote the polymer to form a thicker and more uniform carbon layer, which combines with the generated transition metal oxide to form a stable and dense physical barrier, isolating mass transfer, heat transfer and smoke escape, and greatly enhancing the flame retardant and smoke suppression efficiency of PLA;

[0019] (2) The present invention can significantly improve the hydrophobicity of the flame retardant by in-situ coating the copper lignin sulfonate-polyphosphazene layer on the surface of the MXene nanosheet, thereby facilitating the improvement of the compatibility between the flame retardant and the PLA matrix.

[0020] In summary, the present invention successfully prepared lignin sulfonate copper-polyphosphazene cross-linked modified MXene flame retardant by cross-linking polymerization of lignin sulfonate and phosphazene on the surface of MXene nanosheets and chelating transition metal copper ions. This not only significantly improved the flame retardant properties, but also improved the hydrophobic properties and its compatibility with the PLA matrix, while minimizing the deterioration of the mechanical properties of the PLA matrix caused by the addition of the flame retardant, while improving the flame retardancy and smoke suppression properties of the PLA composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a comparison chart of XRD of MXene and MXene / CLS-PZS prepared in Example 1;

[0022] like Figure 1As shown in the figure, for MXene, characteristic diffraction peaks corresponding to (002), (004), (008), and (110) can be observed near 2θ=8.9°, 16.3°, 27.4°, and 34.1° in the XRD spectrum, which are consistent with the standard card of titanium aluminum carbide (JCPDS 52-0875), and the (104) peak at 2θ=39.1° disappears, corresponding to the Al peak in Ti3AlC2, indicating that the A layer in the MAX phase was successfully removed by etching; while the XRD spectrum of MXene / CLS-PZS contains the above-mentioned characteristic diffraction peaks of (002), (004), (008), and (110), indicating that MXene / CLS-PZS still has a typical MXene-like crystal structure, but the peak surface becomes wider and the peak intensity becomes weaker, which is attributed to the copper lignin sulfonate-polyphosphorus acid After nitrile cross-linking coating, the crystallinity becomes weaker; in addition, compared with the XRD spectrum of MXene, the XRD spectrum of MXene / CLS-PZS shows that the (002) characteristic peak shifts to a smaller 2θ angle to 2θ=8.7°. According to the Bragg equation 2dsinθ=nλ, a smaller 2θ corresponds to a wider interplanar spacing, indicating that after surface polymerization of copper lignin sulfonate-polyphosphazene, the interlayer spacing of MXene / CLS-PZS nanosheets increases, and the agglomeration phenomenon between nanosheets is suppressed, which is beneficial to the dispersion of flame retardants in the matrix.

[0023] Figure 2 It is a FT-IR comparison chart of MXene and MXene / CLS-PZS prepared in Example 1;

[0024] like Figure 2 As shown in Figure 2, the FT-IR spectra of MXene and MXene / CLS-PZS are between 3400 and 3500 cm -1 There are broad vibration peaks at 2921cm, which correspond to the stretching vibration of the hydroxyl group (ν-OH) on the MXene surface and in the CLS molecular structure. -1 The vibration peak that appears is the stretching vibration of the CH bond, at 1630cm -1 The characteristic peak at 655cm corresponds to the stretching vibration of the C=O bond. -1 The characteristic peak at 1586cm corresponds to the stretching vibration of Ti-O bond in MXene. Compared with the FT-IR of MXene, the infrared spectrum of MXene / CLS-PZS shows the following new characteristic peaks: -1 and 1509cm -1 The characteristic absorption peak at 960 cm -1 The characteristic peak at 1214 cm -1 and 1062cm -1The characteristic peak at 835cm belongs to the stretching vibration of P=N on the phosphazene ring. -1 The stretching vibration peak of PN is at 1113cm -1 and 1037cm -1 The characteristic absorption peaks at correspond to the symmetric and antisymmetric stretching vibrations of S=O in the sulfonic acid group. The newly appeared characteristic vibration peaks prove the existence of lignin sulfonate and phosphazene rings, indicating that HCCP and CLS have undergone a condensation reaction. Combined with XRD spectral analysis, it is concluded that through nucleophilic substitution reaction, copper lignin sulfonate-polyphosphazene undergoes cross-linking polymerization, increasing the interlayer spacing while forming an organic copolymer containing N / P / S elements.

[0025] Figure 3 It is a SEM and TEM comparison picture of MXene and MXene / CLS-PZS prepared in Example 1;

[0026] like Figure 3 As shown in the figure, it can be observed from the SEM images (A and B) and TEM (F) of MXene that the MXene prepared by etching has a typical two-dimensional layered nanosheet structure, with a relatively smooth surface and a high degree of etching and peeling. As for MXene / CLS-PZS, its SEM images (C and D) and TEM (G and H) show that MXene / CLS-PZS also maintains a two-dimensional layered structure similar to MXene, but the surface of the nanosheet becomes rough and is covered by a layer of material, which is attributed to the cross-linked coating generated by the polymerization of copper lignin sulfonate and phosphazene on the surface of MXene. The rough surface increases the contact area, which is conducive to the enhancement of interfacial interactions and thus improves the compatibility and dispersibility of the flame retardant in the PLA matrix; the high-resolution TEM (I) of MXene / CLS-PZS calculates that the interplanar spacing is 0.32nm, corresponding to the diffraction peak of 2θ=27.8°(008), which is consistent with the XRD results; through EDS The mapping analysis of the elements contained in MXene / CLS-PZS (E) showed that MXene / CLS-PZS contained C, N, O, Ti, P, S, and Cu elements, of which N and P elements came from hexachlorocyclotriphosphazene, S element came from lignin sulfonate, and Cu indicated the chelation of copper ions; it can be concluded that without changing the two-dimensional layered structure, lignin sulfonate and phosphazene cross-linked and polymerized on the surface of MXene and chelated copper ions to form a layer of CLS-PZS copolymer to coat MXene and increase its interlayer distance, while introducing N, P, S flame retardant elements and Ti, Cu transition metal elements, so that it can play a synergistic flame retardant and catalytic carbonization role in condensed phase and gas phase flame retardancy. .

[0027] Figure 4MXene and MXene / CLS-PZS prepared in Example 1 are water contact angle diagrams;

[0028] like Figure 4 As shown in the figure, generally speaking, the lower the WCA value of a material, the stronger its hydrophilicity, and the higher the WCA value, the stronger its hydrophobicity; the water contact angle of MXene is 7.8°, while the water contact angle of MXene / CLS-PZS increases to 50.5°. The water contact angle of MXene is extremely low, and it is an extremely hydrophilic material. The water contact angle of MXene / CLS-PZS flame retardant increases significantly, indicating that its hydrophobicity has been significantly improved, because a layer of hydrophobic phosphazene-lignin sulfonate copper is coated on the hydrophilic surface of MXene to replace most of the hydroxyl groups. The significantly improved hydrophobicity of MXene / CLS-PZS is conducive to better compatibility and dispersion of the flame retardant in the PLA matrix, thereby significantly improving the tensile strength and toughness of the PLA composite material. At the same time, the flame retardant that is evenly dispersed during combustion can better play a physical barrier role, improve the density and uniformity of the carbon layer, and have a better flame retardant effect in the condensed phase.

[0029] Figure 5 It is a cross-sectional SEM image of PLA / MXene and PLA / MXene / CLS-PZS composite materials prepared by melt blending of pure PLA, MXene and MXene / CLS-PZS prepared in Example 1;

[0030] like Figure 5As shown in the figure, the microstructures of the liquid nitrogen brittle fracture sections of pure PLA, PLA / MXene and PLA / MXene / CLS-PZS composites are compared. The cross section of pure PLA is smooth, and some cracks appear under the stress of brittle fracture. After adding MXene flame retardant to PLA, the two-dimensional layered structure of MXene nanosheets can be clearly observed in the SEM of the cross section of PLA / MXene composites. Due to its own easy stacking and agglomeration characteristics, MXene is dispersed unevenly in PLA and there is a relatively obvious interface between the two, indicating that MXene and PLA have poor compatibility, which will have a negative impact on the mechanical properties and flame retardancy of PLA composites. The dispersion and compatibility of the e / CLS-PZS flame retardant in PLA are satisfactory: by observing the fracture cross-section SEM of the PLA / MXene / CLS-PZS composite material, it is not difficult to see that there is almost no interface between the flame retardant MXene / CLS-PZS and the PLA matrix, and the two seem to have merged into one. The cross-linking and coating of the MXene surface with a layer of CLS-PZS can significantly improve the dispersion and compatibility of MXene / CLS-PZS in PLA, which is beneficial to enhancing the mechanical properties of the PLA / MXene / CLS-PZS composite material, and at the same time enable the flame retardant to better play the role of a physical barrier, combined with the carbon layer to effectively block heat and oxygen transfer, and enhance the flame retardant and smoke suppression capabilities.

[0031] Figure 6 These are digital photos and SEM images of carbon residues of PLA / MXene and PLA / MXene / CLS-PZS composite materials prepared by melt blending of pure PLA, MXene and MXene / CLS-PZS prepared in Example 1 after CCT testing;

[0032] like Figure 6As shown in the figure, the digital photo of the residual carbon shows that almost no coke is left after the combustion of PLA, which cannot block the mass transfer and heat transfer during combustion; while the residual carbon after the combustion of PLA / MXene is loose and of low density, with honeycomb-like holes on the surface and a white appearance, indicating that titanium carbide is oxidized into anatase during combustion, and the loose carbon layer cannot effectively block the transfer of heat and oxygen and the escape of smoke; the carbon layer of the PLA / MXene / CLS-PZS composite material appears continuous and dense, with a uniform surface and no voids. The SEM image shows that the char residue after the combustion of PLA cannot form a physical barrier to protect the PLA matrix. Although the size and thickness of the char residue formed by PLA / MXene are improved, its microstructure is composed of scattered and disordered nanosheets. This is caused by the poor dispersion of MXene in PLA and its own agglomeration. The formed carbon layer is unevenly distributed and has holes and defects. It cannot form a dense and stable physical barrier, and naturally cannot achieve satisfactory flame retardant and smoke suppression effects. In comparison, according to the SEM image of the char residue of the PLA / MXene / CLS-PZS composite material, it can be observed that the generated char residue is very uniform, forming a dense, continuous and hole-free char layer with a certain thickness, which plays a flame retardant role in the condensed phase and significantly improves the flame retardant and smoke suppression efficiency of the PLA composite material. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with embodiments.

[0034] MXene is obtained by etching Ti3AlC2:

[0035] First, 1g of Ti3AlC2 powder was slowly added to a plastic beaker containing 20mL of 50% pure HF solution using a plastic medicine spoon and magnetically stirred at room temperature for 24h. Subsequently, the reacted solution was centrifuged several times at 5000rpm until the pH of the suspension was >6. After adding a certain amount of deionized water and ultrasonicating for 20min, the obtained solid was washed with deionized water and filtered. Finally, the solid obtained after filtration was dried at 80°C for 8h and then ground to obtain MXene powder and sealed for storage.

[0036] Example 1

[0037] (1) 1 g of MXene was weighed and dissolved in 300 mL of deionized water, and then ultrasonicated in an ice bath for 30 min to make it uniformly dispersed. Then, 40 mL of 3-aminopropyltriethoxysilane (APTES) was added dropwise thereto. After magnetic stirring for 1 h, the mixture was centrifuged, washed and dried to obtain silanized MXene.

[0038] (2) 1 g of silanized MXene and 0.15 g of sodium lignin sulfonate (SLS) were added to a three-necked flask containing 100 mL of acetonitrile and ultrasonically treated for 0.5 h. After the reactants were evenly dispersed, 0.1 g of hexachlorotriphosphazene (HCCP) was dissolved in 100 mL of acetonitrile and slowly added dropwise to the above slurry. At the same time, 15 mL of triethylamine (TEA) was added. Under a nitrogen atmosphere, a heat-collecting constant temperature heating magnetic stirrer was used to keep the reaction at 40 °C for 12 h. After the reaction was cooled to room temperature, the sample was washed with acetonitrile and deionized water, filtered with a filter membrane and vacuum dried at 80 °C for 12 h. The dried sample was dispersed in 100 mL of deionized water, and 50 mL of 0.05 M cupric chloride solution was slowly added thereto. The mixture was stirred magnetically for 30 min, washed with deionized water and filtered under reduced pressure with a filter membrane. The filtered sample was vacuum dried at 80 °C for 12 h and ground. The black powder obtained was the copper lignin sulfonate-polyphosphazene cross-linked coated MXene flame retardant, recorded as MXene / CLS-PZS.

[0039] Performance Test:

[0040] By melt blending, the flame retardant prepared in Example 1 (S1) and MXene (D1) was melt blended with PLA to obtain a PLA composite material with a flame retardant mass fraction of 5 wt%, and the flame retardant and mechanical properties were tested. The results are shown in Table 1.

[0041] Table 1 Flame retardant and mechanical properties test results of different PLA composites

[0042]

[0043]

[0044] As shown in Table 1, the tensile strength and elongation at break of pure PLA are 52.7MPa and 5.4%, respectively, showing good elasticity and toughness. With the addition of flame retardants, the tensile strength and elongation at break of the composite material decreased to varying degrees. When 5wt% MXene was added, the tensile strength and elongation at break of PLA / MXene were 48.8MPa and 1.7%, respectively, and its mechanical properties decreased to a large extent. When MXene was modified with CLS-PZS, the mechanical properties were significantly improved, with tensile strength and elongation at break of 50.2MPa and 2.6%, respectively.

[0045] Pure PLA is extremely flammable and has a melting droplet phenomenon in the combustion experiment. Its LOI value is only 19.2. When 5wt% MXene is added, the LOI value is 20.9%, which only passes the UL-94V-2 level. When 5wt% MXene / CLS-PZS is added, the LOI is directly increased to 28.2%, and it reaches the UL-94V-0 level, showing good flame retardant properties.

[0046] The pHRR (peak heat release rate) of pure PLA is 446.4 kW·m -2 , which makes it very easy to burn in the air. After adding different flame retardants, the pHRR of PLA / MXene decreased to 358.4kW·m -2 , while the pHRR of PLA / MXene / CLS-PZS composite material further decreased to 298.6kW·m -2 The THR (total heat release) of pure PLA is 74.9 MJ·m -2 The THR of PLA / MXene is 68.4 MJ·m -2 , while that of PLA / MXene / CLS-PZS composite material was reduced to 62.9 MJ·m -2 It can be seen that MXene / CLS-PZS can significantly improve the flame retardant properties of PLA.

[0047] The smoke released by polymers during combustion will affect the speed of escape and rescue during a fire, so it is also very important to study the smoke suppression performance of polymers. Pure PLA will release a large amount of smoke during combustion, and its TSP (total smoke production) is 24.64m 2 When 5 wt% MXene was added, the TSP of the PLA / MXene composite dropped to 19.08 m 2 After adding MXene / CLS-PZS flame retardant to PLA, the TSP of PLA / MXene / CLS-PZS composite material dropped to 14.31m 2 The smoke release during the combustion process has been significantly controlled and its smoke suppression performance has been significantly improved.

Claims

1. A method for preparing a copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant, characterized in that: The following steps are involved: (1) ultrasonically dispersing MXene in deionized water to obtain a MXene dispersion; adding APTES (3-aminopropyltriethoxysilane) to the MXene dispersion, stirring and mixing, and obtaining silanized MXene after solid-liquid separation; (2) The silanized MXene and sodium lignin sulfonate (SLS) are ultrasonically dispersed in acetonitrile to obtain a mixed slurry; hexachlorotripolyphosphazene (HCCP) is ultrasonically dispersed in acetonitrile to obtain a hexachlorotripolyphosphazene solution; the hexachlorotripolyphosphazene solution and triethylamine (TEA) are simultaneously added dropwise to the mixed slurry, heated and stirred for reaction, and the solid sample obtained after solid-liquid separation is ultrasonically dispersed in deionized water, and copper chloride solution is added dropwise thereto, and the mixture is thoroughly stirred to obtain copper lignin sulfonate-polyphosphazene cross-linked modified MXene flame retardant, which is recorded as MXene / CLS-PZS.

2. The preparation method according to claim 1, characterized in that: In step (1), the concentration of the MXene dispersion is 0.2-0.5 g:100 ml.

3. The preparation method according to claim 1, characterized in that: In step (1), the mass volume ratio of MXene and APTES is 1 g: 30-50 ml.

4. The preparation method according to claim 1, characterized in that: In step (2), the amounts of silylated MXene, sodium lignin sulfonate, hexachlorotriphosphazene and triethylamine are 1 g: 0.1-0.3 g: 0.05-0.2 g: 10-30 ml.

5. The preparation method according to claim 1, characterized in that: In step (2), the heating temperature is 30 to 50° C. and the reaction time is 8 to 24 hours.

6. The copper sulfonate-polyphosphazene cross-linked modified MXene flame retardant prepared by the preparation method according to any one of claims 1 to 5.

Citation Information

Cited By

  • Preparation method of water-soluble polyamino phosphorus-nitrogen compound modified titanium carbide compound

    CN120005281A