Modified polypropylene cable insulation material and preparation method thereof

Through the preparation of modified polypropylene cable insulating material, combined with the use of impact-resistant copolymerized polypropylene and multifunctional additives, the problem of insufficient toughness and aging resistance of high-voltage DC cable materials is solved, and the environmental protection, recycling and performance improvement of the material is achieved .

CN119019785AInactive Publication Date: 2024-11-26HUNAN BOYUDA TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411172860.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN119019785A_ABST
    Figure CN119019785A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cable materials, and discloses a modified polypropylene cable insulation material and a preparation method thereof. The modified polypropylene cable insulation material is prepared from the following components in parts by weight: 30 to 70 parts of impact-resistant co-polypropylene, 20 to 50 parts of isotactic polypropylene, 1 to 3.5 parts of multifunctional additive and 0.1 to 0.2 part of lubricant. The modified polypropylene cable insulation material disclosed by the invention has excellent dielectric property, toughness and thermal oxidation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cable materials, in particular to a modified polypropylene cable insulating material and a preparation method thereof. Background Art

[0002] In terms of high-voltage direct current transmission, cross-linked polyethylene has become the main insulating material for high-voltage direct current cables due to its good physical and chemical properties and dielectric properties. However, there are many problems with the manufacture and use of cross-linked polyethylene cables: the cross-linking process of cross-linked polyethylene is complicated, the cross-linking equipment occupies a large space, the production efficiency is not high, and a variety of by-products such as acetophenone and cumyl alcohol are produced during the cross-linking process. On the one hand, the cross-linking by-products exist in the cable in the form of impurities. On the other hand, under the action of the electric field, the by-products are ionized into ion pairs, forming space charge accumulation inside the material. Moreover, cross-linked polyethylene is a thermosetting material and cannot be recycled later. There is also the problem of environmental pollution.

[0003] Therefore, it is necessary to study a new type of environmentally friendly, recyclable, and cross-link-free insulating material to replace cross-linked polyethylene in order to improve the problems of existing cables. Polypropylene, as a widely used thermoplastic material, has excellent performance in heat resistance, insulation and mechanical strength. It does not require cross-linking during manufacturing and can be recycled. However, polypropylene does not meet the requirements of high-voltage DC cable insulation materials due to its poor toughness and poor aging resistance. In order to give polypropylene flexibility, polypropylene-based blends are generally designed by adding fillers. However, this method often leads to a decrease in its dielectric properties. Therefore, how to improve the comprehensive performance of polypropylene materials is crucial. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a modified polypropylene cable insulation material, which comprises the following components by weight: 30-70 parts of impact copolymer polypropylene, 20-50 parts of isotactic polypropylene, 1-3.5 parts of multifunctional additives, and 0.1-0.2 parts of lubricants;

[0005] Wherein, the multifunctional additive is prepared by the following method:

[0006] Step S1, catalytically oxidizing aminoethanol to obtain 2-aminoacetaldehyde;

[0007] Step S2, modifying the carbon nanohorns by 2-aminoacetaldehyde to obtain modified carbon nanohorns;

[0008] Step S3, reacting the modified carbon nanohorn with 2,6-di-tert-butylphenol to obtain an intermediate B;

[0009] Step S4: intermediate B reacts with methacrylic acid to obtain a multifunctional additive.

[0010] Preferably, the preparation method of the impact-resistant copolymer polypropylene is as follows: at 65-75° C., vacuuming and purging with nitrogen for 2-4 cycles, introducing 0.28-0.32 MPa of hydrogen into the reactor, and then adding ethylene; mixing 0.5 mol / L triethylaluminum heptane dispersion, 0.1 mol / L diisopropyldimethoxysilane heptane dispersion, 0.5 mol / L 5-hexenylmethyldichlorosilane heptane dispersion, and a composite catalyst, and injecting them into the reactor together with liquid propylene, heating to 65-75° C., reacting for 50-70 minutes, and ending the first stage reaction; introducing 1.5-1.7 MPa of equimolar ratio ethylene / propylene mixed gas into the reactor, adjusting the temperature to 65-75° C., and starting the second stage reaction, measuring the gas consumption, when the second stage ethylene / propylene copolymerization is 177.0 g, cutting off the gas supply and releasing the pressure in the reactor, recovering white particles, stirring the white particles for hydrolysis, and then drying;

[0011] Furthermore, the content of each component in the composite catalyst is: 16.83wt% of titanium tetrachloride, 11.53wt% of 9,9-bis(methoxymethyl)fluorene, and the rest is magnesium chloride; the usage ratio of ethylene, heptane dispersion of triethylaluminum, heptane dispersion of diisopropyldimethoxysilane, heptane dispersion of 5-hexenylmethyldichlorosilane, composite catalyst, and liquid propylene is (5-10)g:(5-10)mL:(1-2)mL:(1.9-3.8)mL:(0.014-0.028)g:(1.0-2.0)kg;

[0012] Furthermore, the white particles are stirred and hydrolyzed under the following conditions: stirring and hydrolyzing at 95-105° C. for 15-25 min;

[0013] In the above process, the preparation of impact copolymer polypropylene is divided into two stages of reaction. In the first stage, ethylene is added to the polypropylene matrix, and in the second stage, ethylene / propylene copolymer is added to the polypropylene matrix. In addition, a multi-branched long chain structure is introduced through 5-hexenylmethyldichlorosilane during the reaction.

[0014] Preferably, in step S1, the preparation method of 2-aminoacetaldehyde is as follows: at room temperature, equal volumes of a saturated hydrochloric acid solution in diethyl ether and a chloroform solution in N-methylmorpholine are mixed,

[0015] The mixture is stirred until uniform to obtain a reaction mixture, wherein the molar ratio of hydrochloric acid to N-methylmorpholine is controlled to be 1:(0.9-1.1); the reaction mixture is cooled to 0-5° C., and then chromium trioxide is added three times, stirred for 10-20 minutes, and then aminoethanol is added, and microwave reaction is performed at 55-65° C. for 5-10 minutes. The obtained reaction product is purified by a silica gel column to obtain 2-aminoacetaldehyde; wherein the amount ratio of the reaction mixture, chromium trioxide, and aminoethanol is (100-200) mL:(18-54) g:(20-40) g;

[0016] In the above process, an N-methylmorpholine chlorochromate catalyst is generated using N-methylmorpholine, hydrochloric acid and chromium trioxide as raw materials. The catalyst is used to catalyze the oxidation of aminoethanol under the assistance of microwaves, which greatly improves the reaction efficiency. 2-aminoacetaldehyde can be obtained within 10 minutes, and the formation of toxic and harmful chromium chloride is avoided.

[0017] Preferably, in step S2, the preparation method of the modified carbon nanohorn is as follows: in an argon atmosphere, carbon nanohorns and 2-aminoacetaldehyde are added to o-dichlorobenzene, ultrasonically treated for 20-40 minutes, and then isoamyl nitrite is added, sealed, and irradiated with 10W light for 3-5 times at 150-170°C, each irradiation for 8-10 seconds. After the reaction is completed, the reaction mixture is cooled to room temperature, and the reaction mixture is diluted with N,N-dimethylformamide, filtered, and washed to obtain the modified carbon nanohorn; wherein the amount ratio of carbon nanohorns, 2-aminoacetaldehyde, o-dichlorobenzene, and isoamyl nitrite is (12-24) g: (0.4-1.2) g: (400-700) mL: (500-800) mL;

[0018] In the above process, 2-aminoacetaldehyde is anchored on the nanohorn through its own amino group, and an aldehyde group is introduced on the surface of the carbon nanohorn.

[0019] Preferably, in step S3, the preparation method of the intermediate B is as follows: tert-butyl alcohol, modified carbon nanohorns and potassium tert-butylate are mixed and stirred until uniform to obtain a mixed solution A; 2,6-di-tert-butylphenol and tert-butyl alcohol are mixed, stirred under a nitrogen atmosphere, heated to 45-55° C., and then the mixed solution A is dripped within 40-60 minutes, the temperature is kept constant, the reaction is stirred for 100-150 minutes, filtered, washed, and dried to obtain an intermediate B; wherein the mass ratio of modified carbon nanohorns, potassium tert-butylate and 2,6-di-tert-butylphenol is (8.7-17.4):(0.3-0.5):(10-20);

[0020] In the above process, the carbon-hydrogen bond at the para position of the phenolic hydroxyl group in 2,6-di-tert-butylphenol reacts with the aldehyde group in the modified carbon nanohorn to generate an alcoholic hydroxyl group, thereby introducing the 2,6-di-tert-butylphenol structure into the surface of the carbon nanohorn.

[0021] Preferably, in step S4, the preparation method of the multifunctional additive is as follows: methacrylic acid, benzene, hydroquinone and p-toluenesulfonic acid are mixed, stirred and heated to 38-42° C. in a nitrogen atmosphere, then intermediate B is added, the temperature is raised to 75-85° C. and the reaction is performed for 100-150 min, then a 5 wt % sodium carbonate aqueous solution is added and stirred, and purified to obtain a multifunctional additive; wherein the amount ratio of methacrylic acid, benzene, hydroquinone, p-toluenesulfonic acid and intermediate B is (10-20) g: (80-200) mL: (0.02-0.04) g: (0.5-0.8) g: (9-15) g;

[0022] In the above process, the carboxyl group of methacrylic acid undergoes an esterification reaction with the alcoholic hydroxyl group of the intermediate B to obtain a multifunctional additive.

[0023] The invention also discloses a method for preparing a modified polypropylene cable insulation material, comprising the following steps: weighing impact-resistant copolymer polypropylene, isotactic polypropylene, multifunctional additives and lubricant in proportion, mixing them evenly, and then melt-extruding them through a twin-screw extruder, water-cooling and pelletizing them to obtain the modified polypropylene insulation cable material.

[0024] Preferably, the rotation speed of the twin-screw extruder is 150-300 r / min, the reaction temperature is 180-220° C., and the extruder die filter is 60-500 mesh.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. In the process of preparing impact-resistant copolymer polypropylene, ethylene is introduced in the first reaction stage to adjust the chain structure of the polypropylene matrix, reduce the average sequence length of the polypropylene chain, and improve the mechanical flexibility; more importantly, the ethylene structure incorporated into the polypropylene matrix can narrow the structural gap between the polypropylene and the ethylene / propylene copolymer, improve their interface compatibility, and promote the formation of a large number of deep electron traps, thereby improving the toughness and dielectric properties of the polypropylene material; in addition, the toughness and dielectric properties of the polypropylene material are further improved by introducing a multi-branched long chain structure.

[0027] 2. The present invention uses carbon nanohorns as a matrix of a multifunctional additive, and then modifies it to introduce aldehyde groups, and then reacts with 2,6-di-tert-butylphenol to generate an intermediate B, and the intermediate B reacts with methacrylate to perform an esterification reaction, and performs surface organic treatment on the carbon nanohorns to obtain a multifunctional additive; the carbon nanohorns as a matrix can be evenly and stably dispersed in the polypropylene cable material due to their own special structure, inhibiting the accumulation of space charges and improving the insulation of the polypropylene cable material; performing surface organic treatment on the carbon nanohorns can not only improve the dispersibility of the carbon nanohorns, but also chemically fix the organic components of the carbon nanohorns to avoid the migration of the organic components, and more importantly, after the surface organic treatment, the carbon nanohorns can be The acrylate structure introduced on the surface contains reactive groups, which can quickly capture free radicals in the initial stage, and the large tert-butyl group of 2,6-di-tert-butylphenol is an electron-donating group. The hydroxyl group in the multifunctional additive has strong reactivity and can quickly combine with free radicals to prevent the free radicals from damaging the polypropylene cable material, thereby improving the thermal oxidation resistance of the polypropylene cable material and broadening the working temperature range of the cable material; further, surface organic treatment of the carbon nanohorns can inhibit the formation of cracks and hinder the development of cracks, thereby improving the toughness of the polypropylene cable material system; therefore, the multifunctional additive of the present invention has multiple effects of improving the dielectric properties, toughness and thermal oxidation resistance of the polypropylene cable material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a comparison chart of oxidation induction temperature test of modified polypropylene insulation materials of Examples 3-5 of the present invention and Comparative Examples 5-9;

[0029] Figure 2 It is a comparison chart of tensile strength test of modified polypropylene insulating materials of Examples 3-5 of the present invention and Comparative Examples 5-9;

[0030] Figure 3 It is a comparison chart of the impact strength test of the modified polypropylene insulating material of Examples 3-5 of the present invention and Comparative Examples 5-9;

[0031] Figure 4 It is a comparison chart of the breakdown strength test of the modified polypropylene insulation material of Examples 3-5 of the present invention and Comparative Examples 5-9. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] This embodiment discloses a method for preparing a multifunctional additive, comprising the following steps:

[0035] Step S1, at room temperature, mixing equal volumes of a saturated hydrochloric acid solution in ether and a N-methylmorpholine solution in chloroform, stirring until uniform, to obtain a reaction mixture, wherein the molar ratio of hydrochloric acid to N-methylmorpholine is controlled to be 1:1; cooling the reaction mixture to 3° C., then adding chromium trioxide three times, stirring for 15 minutes, then adding aminoethanol, reacting at 60° C. by microwave for 8 minutes, and purifying the obtained reaction product by a silica gel column to obtain 2-aminoacetaldehyde; wherein the amount ratio of the reaction mixture, chromium trioxide, and aminoethanol is 150 mL:36 g:30 g.

[0036] Step S2, in an argon atmosphere, 18 g of carbon nanohorns and 0.8 g of 2-aminoacetaldehyde were added to 600 mL of o-dichlorobenzene, and ultrasonic treatment was performed for 30 min. Then, 650 mL of isoamyl nitrite was added, and the mixture was sealed. At 160° C., 10 W light was irradiated for 4 times, each time for 10 seconds. After the reaction was completed, the mixture was cooled to room temperature, and the reaction mixture was diluted with N,N-dimethylformamide, filtered, and washed to obtain modified carbon nanohorns.

[0037] Step S3, 120 mL of tert-butanol, 13 g of modified carbon nanohorns, and 0.4 g of potassium tert-butoxide are mixed and stirred until uniform to obtain a mixed solution A; 15 g of 2,6-di-tert-butylphenol and 150 mL of tert-butanol are mixed, stirred under a nitrogen atmosphere, heated to 50° C., and then the mixed solution A is dripped within 50 minutes, the temperature is kept unchanged, the reaction is stirred for 120 minutes, filtered, washed, and dried to obtain an intermediate B.

[0038] Step S4, 15g of methacrylic acid, 150mL of benzene, 0.03g of hydroquinone, and 0.7g of p-toluenesulfonic acid are mixed, stirred and heated to 40°C in a nitrogen atmosphere, and then 12g of intermediate B is added, the temperature is raised to 80°C and reacted for 120min, and then 5wt% sodium carbonate aqueous solution is added and stirred to remove the inhibitor hydroquinone and unreacted methacrylic acid, and purified to obtain a multifunctional additive.

[0039] Example 2

[0040] The present embodiment discloses a method for preparing an impact copolymer polypropylene, comprising the following steps: at 70° C., repeatedly evacuating and purging a reactor with a volume of 5 L with nitrogen for three cycles, introducing 0.3 MPa of hydrogen into the reactor, and then adding 7.5 g of ethylene; mixing 7.5 mL of a 0.5 mol / L heptane dispersion of triethylaluminum, 1.5 mL of a 0.1 mol / L heptane dispersion of diisopropyldimethoxysilane, and 2.7 mL of a 0.5 mol / L A heptane dispersion of 5-hexenylmethyldichlorosilane and 0.021g of a composite catalyst are mixed and injected into a reactor together with 1.5kg of liquid propylene, and the temperature is raised to 70°C. After the reaction for 60 minutes, the first stage reaction ends; 1.6MPa of an equimolar ratio ethylene / propylene mixed gas is introduced into the reactor, the temperature is adjusted to 70°C, and the second stage reaction begins, which is measured by gas consumption. When the second stage ethylene / propylene copolymerization reaches 177.0g, the gas supply is cut off and the pressure in the reactor is released, white particles are recovered, and the white particles are stirred and hydrolyzed at 100°C for 20 minutes in a steam autoclave, and vacuum dried at 65°C for 25 hours to obtain impact-resistant copolymerized polypropylene; wherein the contents of the components in the composite catalyst are: 16.83wt% of titanium tetrachloride, 11.53wt% of 9,9-bis(methoxymethyl)fluorene, and the rest is magnesium chloride.

[0041] Example 3

[0042] This embodiment discloses a method for preparing a modified polypropylene cable insulation material, comprising the following steps:

[0043] In parts by weight, 30 parts of the impact copolymer polypropylene prepared in Example 2, 20 parts of isotactic polypropylene, 1 part of the multifunctional additive prepared in Example 1, and 0.1 part of the lubricant are mixed evenly, and then melt-extruded, water-cooled, and pelletized through a twin-screw extruder to obtain a modified polypropylene insulated cable material; wherein the speed of the twin-screw extruder is 150r / min, the reaction temperature is 180°C, and the extruder die filter is 60 mesh.

[0044] Example 4

[0045] This embodiment discloses a method for preparing a modified polypropylene cable insulation material, comprising the following steps:

[0046] In parts by weight, 70 parts of the impact copolymer polypropylene prepared in Example 2, 50 parts of isotactic polypropylene, 3.5 parts of the multifunctional additive prepared in Example 1, and 0.2 parts of the lubricant are mixed evenly, and then melt-extruded, water-cooled, and pelletized through a twin-screw extruder to obtain a modified polypropylene insulated cable material; wherein the speed of the twin-screw extruder is 300 r / min, the reaction temperature is 220°C, and the extruder die filter is 500 mesh.

[0047] Example 5

[0048] This embodiment discloses a method for preparing a modified polypropylene cable insulation material, comprising the following steps:

[0049] In parts by weight, 50 parts of the impact copolymer polypropylene prepared in Example 2, 35 parts of isotactic polypropylene, 2.5 parts of the multifunctional additive prepared in Example 1, and 0.15 parts of the lubricant are mixed evenly, and then melt-extruded, water-cooled, and pelletized through a twin-screw extruder to obtain a modified polypropylene insulated cable material; wherein the speed of the twin-screw extruder is 250r / min, the reaction temperature is 200°C, and the extruder die filter is 300 mesh.

[0050] Comparative Example 1

[0051] This comparative example discloses a method for preparing a multifunctional additive, comprising the following steps:

[0052] Step S1, at room temperature, mixing equal volumes of a saturated hydrochloric acid solution in ether and a N-methylmorpholine solution in chloroform, stirring until uniform, to obtain a reaction mixture, wherein the molar ratio of hydrochloric acid to N-methylmorpholine is controlled to be 1:1; cooling the reaction mixture to 3° C., then adding chromium trioxide three times, stirring for 15 minutes, then adding aminoethanol, reacting at 60° C. by microwave for 8 minutes, and purifying the obtained reaction product by a silica gel column to obtain 2-aminoacetaldehyde; wherein the amount ratio of the reaction mixture, chromium trioxide, and aminoethanol is 150 mL:36 g:30 g.

[0053] Step S2, 120 mL of tert-butanol, 13 g of 2-aminoacetaldehyde, and 0.4 g of potassium tert-butoxide are mixed and stirred until uniform to obtain a mixed solution A; 15 g of 2,6-di-tert-butylphenol and 150 mL of tert-butanol are mixed, stirred under a nitrogen atmosphere, heated to 50° C., and then the mixed solution A is dripped within 50 minutes, the temperature is kept unchanged, the reaction is stirred for 120 minutes, filtered, washed, and dried to obtain an intermediate B.

[0054] Step S3, 15g of methacrylic acid, 150mL of benzene, 0.03g of hydroquinone, and 0.7g of p-toluenesulfonic acid are mixed, stirred and heated to 40°C in a nitrogen atmosphere, and then 12g of intermediate B is added, the temperature is raised to 80°C and reacted for 120min, and then 5wt% sodium carbonate aqueous solution is added and stirred to remove the inhibitor hydroquinone and unreacted methacrylic acid, and purified to obtain a multifunctional additive.

[0055] Comparative Example 2

[0056] This comparative example discloses a method for preparing a multifunctional additive, comprising the following steps:

[0057] Step S1, at room temperature, mixing equal volumes of a saturated hydrochloric acid solution in ether and a N-methylmorpholine solution in chloroform, stirring until uniform, to obtain a reaction mixture, wherein the molar ratio of hydrochloric acid to N-methylmorpholine is controlled to be 1:1; cooling the reaction mixture to 3° C., then adding chromium trioxide three times, stirring for 15 minutes, then adding aminoethanol, reacting at 60° C. by microwave for 8 minutes, and purifying the obtained reaction product by a silica gel column to obtain 2-aminoacetaldehyde; wherein the amount ratio of the reaction mixture, chromium trioxide, and aminoethanol is 150 mL:36 g:30 g.

[0058] Step S2, in an argon atmosphere, 18 g of carbon nanohorns and 0.8 g of 2-aminoacetaldehyde were added to 600 mL of o-dichlorobenzene, and ultrasonic treatment was performed for 30 min. Then, 650 mL of isoamyl nitrite was added, and the mixture was sealed. At 160° C., 10 W light was irradiated for 4 times, each time for 10 seconds. After the reaction was completed, the mixture was cooled to room temperature, and the reaction mixture was diluted with N,N-dimethylformamide, filtered, and washed to obtain modified carbon nanohorns.

[0059] Step S3, 120 mL of tert-butanol, 13 g of modified carbon nanohorns, and 0.4 g of potassium tert-butoxide are mixed and stirred until uniform to obtain a mixed solution A; 15 g of 2,6-di-tert-butylphenol and 150 mL of tert-butanol are mixed, stirred under a nitrogen atmosphere, heated to 50° C., and then the mixed solution A is dripped within 50 minutes, the temperature is kept constant, the reaction is stirred for 120 minutes, filtered, washed, and dried to obtain an intermediate B, i.e., a multifunctional additive.

[0060] Comparative Example 3

[0061] Compared with Example 2, in Comparative Example 3, no ethylene was added in the first stage reaction during the preparation of impact copolymer polypropylene, and other conditions remained unchanged.

[0062] Comparative Example 4

[0063] Comparative Example 4 Compared with Example 2, in the process of preparing the impact-resistant copolymer polypropylene, no 5-hexenylmethyldichlorosilane was added in Comparative Example 4, and other conditions remained unchanged.

[0064] Comparative Example 5

[0065] Comparative Example 5 Compared with Example 5, Comparative Example 5 adopts the multifunctional additive prepared in Comparative Example 1, and other conditions remain unchanged.

[0066] Comparative Example 6

[0067] Compared with Example 5, Comparative Example 6 adopts the multifunctional additive prepared in Comparative Example 2, and other conditions remain unchanged.

[0068] Comparative Example 7

[0069] Compared with Example 5, in Comparative Example 7, carbon nanohorns are used to replace the modified multifunctional additive during the preparation of modified polypropylene cable insulation material, while other conditions remain unchanged.

[0070] Comparative Example 8

[0071] Compared with Example 5, Comparative Example 8 uses the impact-resistant copolymer polypropylene prepared in Comparative Example 3, and other conditions remain unchanged.

[0072] Comparative Example 9

[0073] Compared with Example 5, Comparative Example 9 adopts the impact copolymer polypropylene prepared in Comparative Example 4, and other conditions remain unchanged.

[0074] Experimental example

[0075] The performance tests were performed on the modified polypropylene cable insulation materials of Examples 3-5 and Comparative Examples 5-9.

[0076] 1. Antioxidant performance test: According to the ASTM E 2009-08 measurement procedure, the sample is heated at a heating rate of 10°C / min in an oxygen atmosphere to test the oxidation induction temperature.

[0077] 2. Mechanical properties test:

[0078] 1) The tensile properties were tested on an Instron 3365 universal material testing machine according to GB / T1040.2-2006.

[0079] 2) Impact strength test was carried out on XJC-250 instrument according to GB / T1843-1996. All test samples were injection molded by Haake minijet at 210°C and 800 bar, and the molding machine temperature was 50°C.

[0080] 3. DC breakdown strength test: Using a dielectric strength tester based on IEC-60243-1, a sample with a thickness of approximately 150 μm (±10 μm) was fixed between two spherical electrodes with a diameter of 20 mm to prevent surface flashover, and subjected to a ramp voltage with a step size of 2.2 kV / s until breakdown occurred.

[0081] The test results are shown in Table 1:

[0082] Table 1

[0083] Oxidation induction temperature / ℃ Tensile strength / MPa <![CDATA[Impact strength / (kJ / m 2 )]]> Breakdown strength / (kV / mm) Example 3 288 38.6 53.6 451.7 Example 4 295 39.4 54.4 453.3 Example 5 291 38.9 54.1 452.6 Comparative Example 5 280 38.4 53.3 433.7 Comparative Example 6 282 38.8 53.9 452.4 Comparative Example 7 245 37.9 52.2 449.8 Comparative Example 8 291 37.4 51.6 438.9 Comparative Example 9 290 37.1 51.1 435.2

[0084] From the test results in Table 1, it can be seen that the modified polypropylene cable insulation materials prepared in Examples 2-4 of the present invention have excellent thermal oxidation resistance, toughness and dielectric properties. From the comparison between Comparative Example 5 and Example 5, it can be seen that the addition of carbon nanohorns has different degrees of influence on various properties of polypropylene cable materials, especially the significant influence on dielectric properties; from the comparison between Comparative Examples 6 and 7 and Example 5, it can be seen that the multifunctional additives have an influence on various properties of polypropylene cable materials, and the introduction of methacrylic acid structure mainly affects the thermal oxidation resistance; from the comparison between Comparative Examples 8 and 9 and Example 5, it can be seen that the addition of ethylene and multi-branched long chain structures in the preparation process of impact copolymer polypropylene helps to improve its mechanical and dielectric properties.

[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A modified polypropylene cable insulation material, characterized in that: The composition comprises the following components by weight: 30-70 parts of impact copolymer polypropylene, 20-50 parts of isotactic polypropylene, 1-3.5 parts of multifunctional additives, and 0.1-0.2 parts of lubricants; Wherein, the multifunctional additive is prepared by the following method: Step S1, catalytically oxidizing aminoethanol to obtain 2-aminoacetaldehyde; Step S2, modifying the carbon nanohorns by 2-aminoacetaldehyde to obtain modified carbon nanohorns; Step S3, reacting the modified carbon nanohorn with 2,6-di-tert-butylphenol to obtain an intermediate B; Step S4: intermediate B reacts with methacrylic acid to obtain a multifunctional additive.

2. The modified polypropylene cable insulation material according to claim 1, characterized in that: The preparation method of the impact-resistant copolymer polypropylene comprises the following steps: at 65-75° C., vacuumizing and purging with nitrogen for 2-4 cycles, introducing 0.28-0.32 MPa of hydrogen into the reactor, and then adding ethylene; mixing 0.5 mol / L triethylaluminum heptane dispersion, 0.1 mol / L diisopropyldimethoxysilane heptane dispersion, 0.5 mol / L 5-hexenylmethyldichlorosilane heptane dispersion, and a composite catalyst, and injecting the mixture into the reactor together with liquid propylene, heating to 65-75° C., reacting for 50-70 minutes, and ending the first stage reaction; introducing 1.5-1.7 MPa of equimolar ratio ethylene / propylene mixed gas into the reactor, adjusting the temperature to 65-75° C., and starting the second stage reaction, and measuring the gas consumption when the second stage ethylene / propylene copolymerization temperature is 177.0 118-236 g, the gas supply is cut off and the pressure in the reactor is released, the white particles are recovered, the white particles are stirred and hydrolyzed, and then dried.

3. The modified polypropylene cable insulation material according to claim 2, characterized in that: The content of each component in the composite catalyst is: 16.83wt% of titanium tetrachloride, 11.53wt% of 9,9-bis(methoxymethyl)fluorene, and the rest is magnesium chloride; the dosage ratio of the ethylene, heptane dispersion of triethylaluminum, heptane dispersion of diisopropyldimethoxysilane, heptane dispersion of 5-hexenylmethyldichlorosilane, composite catalyst, and liquid propylene is (5-10)g:(5-10)mL:(1-2)mL:(1.9-3.8)mL:(0.014-0.028)g:(1.0-2.0)kg.

4. The modified polypropylene cable insulation material according to claim 2, characterized in that: The stirring and hydrolysis conditions of the white particles are as follows: stirring and hydrolyzing at 95-105° C. for 15-25 min.

5. The modified polypropylene cable insulation material according to claim 1, characterized in that: In the step S1, the preparation method of 2-aminoacetaldehyde is as follows: at room temperature, saturated hydrochloric acid in ether solution and N-methylmorpholine in chloroform solution are mixed in equal volumes, stirred until uniform, to obtain a reaction mixture, wherein the molar ratio of hydrochloric acid to N-methylmorpholine is controlled to be 1:(0.9-1.1); the reaction mixture is cooled to 0-5°C, and then chromium trioxide is added three times, stirred for 10-20 minutes, and then aminoethanol is added, and microwave reaction is carried out at 55-65°C for 5-10 minutes, and the obtained reaction product is purified by a silica gel column to obtain 2-aminoacetaldehyde; wherein the amount ratio of the reaction mixture, chromium trioxide, and aminoethanol is (100-200) mL:(18-54) g:(20-40) g.

6. The modified polypropylene cable insulation material according to claim 1, characterized in that: In the step S2, the preparation method of the modified carbon nanohorn is as follows: in an argon atmosphere, taking carbon nanohorns and 2-aminoacetaldehyde, adding them to o-dichlorobenzene, ultrasonically treating for 20-40 minutes, then adding isoamyl nitrite, sealing, and irradiating with 10W light for 3-5 times at 150-170°C, each irradiation for 8-10 seconds. After the reaction is completed, cooling to room temperature, diluting the reaction mixture with N,N-dimethylformamide, filtering, and washing to obtain the modified carbon nanohorn; wherein the amount ratio of carbon nanohorns, 2-aminoacetaldehyde, o-dichlorobenzene, and isoamyl nitrite is (12-24) g: (0.4-1.2) g: (400-700) mL: (500-800) mL.

7. The modified polypropylene cable insulation material according to claim 1, characterized in that: In the step S3, the preparation method of the intermediate B is as follows: tert-butyl alcohol, modified carbon nanohorns, and potassium tert-butylate are mixed and stirred until uniform to obtain a mixed solution A; 2,6-di-tert-butylphenol and tert-butyl alcohol are mixed, stirred under a nitrogen atmosphere, heated to 45-55° C., and then the mixed solution A is dripped within 40-60 minutes, the temperature is kept constant, the reaction is stirred for 100-150 minutes, filtered, washed, and dried to obtain an intermediate B; wherein the mass ratio of the modified carbon nanohorns, potassium tert-butylate, and 2,6-di-tert-butylphenol is (8.7-17.4):(0.3-0.5):(10-20).

8. The modified polypropylene cable insulation material according to claim 1, characterized in that: In step S4, the preparation method of the multifunctional additive is as follows: methacrylic acid, benzene, hydroquinone and p-toluenesulfonic acid are mixed, stirred and heated to 38-42° C. in a nitrogen atmosphere, then intermediate B is added, the temperature is raised to 75-85° C. and the reaction is carried out for 100-150 min, then a 5 wt % sodium carbonate aqueous solution is added and stirred, and purified to obtain a multifunctional additive; wherein the amount ratio of methacrylic acid, benzene, hydroquinone, p-toluenesulfonic acid and intermediate B is (10-20) g: (80-200) mL: (0.02-0.04) g: (0.5-0.8) g: (9-15) g.

9. The method for preparing modified polypropylene cable insulation material according to claim 1, characterized in that: The following steps are involved: Impact copolymer polypropylene, isotactic polypropylene, multifunctional additives and lubricant are weighed in proportion, mixed evenly, and then melt-extruded through a twin-screw extruder, water-cooled and pelletized to obtain a modified polypropylene insulating cable material.

10. The method for preparing modified polypropylene cable insulation material according to claim 9, characterized in that: The rotation speed of the twin-screw extruder is 150-300 r / min, the reaction temperature is 180-220° C., and the filter screen of the extruder die is 60-500 meshes.

Citation Information

Cited By

  • Preparation method for and use of modified polypropylene insulating cable material

    WO2026157546A1