Optical fiber preform and method for manufacturing optical fiber preform
By controlling the maximum and minimum values of the refractive index difference within 5% of the inner core radius position of the core glass rod, the problem of cutoff wavelength deviation caused by the refractive index distribution after the diameter of the core gray particles becomes larger is solved. An exact match between the predicted and the actual measured values is achieved.
Patent Information
- Application Number
- CN202380034314.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-10
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, after the diameter of the core gray particles becomes larger, the refractive index distribution of the core glass rod causes a large deviation from the predicted cutoff wavelength and the actual measured cutoff wavelength, especially when the core radius is more than 10 mm. More obvious.
There are maximum and minimum values of relative refractive index differences within 5% of the inner core radius position of the core glass rod, and it is ensured that the difference between the maximum and minimum values ΔM-Δm does not exceed 0.04%, so that In the fiber-core glass rod stage, it is assumed that the additional cladding and the cutoff wavelength is calculated, and the cutoff wavelength is deviated small from the actual cutoff wavelength measured after the actual drawing.
By controlling the refractive index distribution of the fiber core glass rod, ensuring that the value of ΔM-Δm is less than 0.04%, the deviation between the predicted cutoff wavelength and the actual measured cutoff wavelength can be made extremely small, thereby improving the fiber base material manufacturing process Accuracy.
Smart Images

Figure CN119032067A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a refractive index distribution of an optical fiber mother material, wherein the optical fiber mother material is formed into an optical fiber by wire drawing. Background Art
[0002] In recent years, as the amount of data communications has continued to grow, the demand for optical fiber has also increased, and therefore the size of the optical fiber mother material needs to be increased to meet the growing demand.
[0003] The common optical fiber mother material used for communication includes a core part with a high refractive index and a cladding part with a relatively low refractive index located on the periphery thereof. The manufacturing method of the optical fiber mother material includes a two-stage manufacturing method, namely: after manufacturing a core glass rod consisting of a core part and a part of the cladding part, the remaining cladding part is added to the outside of the core glass rod to make the final optical fiber mother material. As a manufacturing method for the core glass rod, the VAD (Vapour Axial Deposition) method is known. In the VAD method, a core deposition burner for depositing a core portion and a cladding deposition burner for depositing a cladding portion on the outside of the core are arranged in a reaction vessel, and glass raw material gas such as silicon tetrachloride, combustible gas such as hydrogen, and combustion-supporting gas such as oxygen are supplied to each burner. After the glass raw material is hydrolyzed in a hydrogen-oxygen flame to generate silica particles, the generated silica particles are rotated with their own central axis as the rotation axis, and are deposited along the central axis starting from a starting part that is elevated relative to the burner, thereby obtaining a porous core soot body including a core layer and a cladding layer. At this time, germanium dioxide is added to the core portion in order to increase the refractive index.
[0004] The obtained core soot particles can be made into core glass rods after transparent vitrification. Specifically, by placing the core soot particles in a processing container and performing a heat treatment using a heater arranged on the outer periphery of the processing container, impurities can be removed and transparent vitrification can be achieved. Here, impurities can be removed by introducing a gas containing chlorine atoms into the ambient gas and heating at a temperature lower than the transparent glass transition temperature of the core soot particles. Impurities to be removed include metal elements and hydroxyl groups (OH groups), which will increase the transmission loss of the optical fiber after drawing. Then, the set temperature of the heater is increased to perform a heat treatment to make the core soot particles into a transparent core glass rod.
[0005] It is expected that the cost of manufacturing a core glass rod can be reduced by increasing the size of the core soot body. For this reason, in the VAD method, by increasing the flow rate of the raw material and the combustible gas supplied to the core deposition burner and the cladding deposition burner, a core soot body with a large diameter can be produced. However, in the case of a core soot body with a larger diameter, when the heater is heated from the periphery as described above, the distance between the surface of the core soot body and the center of the core soot body becomes larger, and therefore, it is necessary to increase the set temperature of the heater so that the center is also sufficiently heated to remove impurities.
[0006] Furthermore, by increasing the set temperature of the heater, germanium dioxide added to the portion near the outer periphery of the core portion is easily volatilized during the heating process, resulting in a change in the refractive index distribution shape of the core glass rod.
[0007] Regarding the measurement of the refractive index distribution of the core glass rod, for example, Non-Patent Document 1 discloses a method for non-destructively measuring the refractive index distribution of the core glass rod, namely, the Refraction Angle Method.
[0008] Figure 1 This is an example of the refractive index distribution of the core glass rod. In addition, the vertical axis is the relative refractive index difference Δ(r) at radius r. The refractive index at radius r is set to n, the refractive index at the core center, that is, when the radius r = 0 is set to n1, and the refractive index of the cladding is set to n2. The relative refractive index difference Δ(r) is calculated by Δ(r) = (n-n2) / n1. Figure 1 The core radius, i.e., the radius position r of 0.45 times the relative refractive index difference at the center 0.45 In addition, the radius r of the center is 0.75 times the relative refractive index difference. 0.75 With r 0.45 R 0.75 / r 0.45 It is 0.921.
[0009] The optical properties of single-mode transmission optical fiber include the cut-off wavelength. The cut-off wavelength is the shortest wavelength that can be propagated in only one mode. It is very important for single-mode transmission optical fiber because it is the boundary between signal light single-mode transmission and multi-mode transmission. The ITU-T Recommendation G.652D standard specifies the upper limit of the cut-off wavelength of optical fiber cables. The cut-off wavelength is mainly affected by the refractive index distribution of the core of the optical fiber.
[0010] Patent Document 1 describes a method for predicting and calculating the cutoff wavelength of an optical fiber based on the refractive index distribution of a base material for an optical fiber, the optical fiber being obtained by drawing the base material. First, the refractive index distribution of the core glass rod is measured, and then the calculation is performed assuming that the remaining cladding portion is already provided, thereby being able to infer the optical characteristics of the final optical fiber at the stage of the core glass rod. [Prior art literature] [Patent Document] [Patent Document 1] Japanese Patent Application Publication No. 2001-281094 [Non-patent literature] [Non-patent document 1] Dietrich Marcuse, "Principles of Optical Fiber Measurements", Academic Press (1981) Summary of the invention
[0011] However, the following phenomenon was discovered: the cutoff wavelength estimated from the refractive index distribution of the core glass rod obtained by transparently vitrifying the core soot particles with a larger diameter deviated greatly from the cutoff wavelength actually measured by drawing the optical fiber mother material with the remaining cladding portion. This phenomenon became particularly obvious when the core radius was 10 mm or more.
[0012] In view of this problem, an object of the present invention is to provide an optical fiber mother material and a method for manufacturing the same, wherein even if the diameter of the core soot particles increases, the deviation between the estimated value obtained by assuming that a cladding is added at the core glass rod stage and estimating the cutoff wavelength and the actual measured value of the cutoff wavelength obtained by actually adding a cladding and drawing is very small.
[0013] After careful research, it was found that there is a point indicating a local high maximum value of the refractive index near the core radius position of the core glass rod, and there is a point indicating a minimum value near it. When the difference between the maximum value and the minimum value is large, the deviation between the estimated value of the cutoff wavelength obtained by assuming that the remaining cladding part is given to the core glass rod and the actual value measured after the cladding part is actually given and drawn is large. Therefore, it was found that when the maximum value of the maximum value of the relative refractive index difference existing in the inner 5% range of the core radius position is set as the maximum value ΔM, and the minimum value is set as the minimum value Δm, if the value of ΔM-Δm does not exceed 0.04%, the deviation between the estimated value and the actual value is small, thereby completing the present invention.
[0014] That is, the optical fiber base material of the present invention is characterized in that: when a core glass base material consisting of a core part and a part of a cladding part is manufactured, and then the remaining cladding part is provided outside the core glass base material, in the core glass base material, a radius position where the relative refractive index difference is 0.45 times the relative refractive index difference at the core center is set as the core radius position, and within 5% of the inner side of the core radius position, there are a point with a maximum value ΔM indicating a local high relative refractive index difference and a point with a minimum value Δm indicating a local low relative refractive index difference, and the value of ΔM-Δm does not exceed 0.04%. In addition, it is characterized in that: the value of ΔM-Δm is preferably not more than 0.03%, more preferably not more than 0.02%, and more preferably not more than 0.01%.
[0015] The manufacturing method of the optical fiber mother material of the present invention is characterized in that it is a method for manufacturing an optical fiber mother material, in which a core glass mother material consisting of a core part and a part of a cladding part is manufactured, and then the remaining cladding part is given to the outside of the core glass mother material; in the core glass mother material, a radius position where the relative refractive index difference is 0.45 times the relative refractive index difference at the core center is set as the core radius position, and within 5% inside the core radius position, there are a point with a maximum value ΔM indicating a locally high relative refractive index difference and a point with a minimum value Δm indicating a locally low relative refractive index difference, and the remaining cladding part is given to the outside of the core glass mother material whose value of ΔM-Δm does not exceed 0.04%.
[0016] According to the present invention, as long as the value of ΔM-Δm calculated based on the refractive index distribution of the core glass rod does not exceed 0.04%, the estimated value of the optical fiber cutoff wavelength obtained by assuming that a cladding is added at the core glass rod stage and estimating the cutoff wavelength is extremely close to the actual measured value obtained by actually adding a cladding and drawing, and a value with extremely small deviation is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a graph showing the relative refractive index difference Δ(r) at radius r. Figure 2 This is a schematic diagram schematically showing the production of a glass particles deposit. Figure 3 It is a schematic diagram showing the cross-sectional shape of the burner for cladding deposition. Figure 4 This is a graph obtained by measuring the refractive index distribution of the core glass rod of Example 1 using a refraction angle method. Figure 5 This is a graph obtained by measuring the refractive index distribution of the core glass rod of Example 6 using a refraction angle method. Figure 6 This is a graph obtained by measuring the refractive index distribution of the core glass rod of Comparative Example 1 using a refraction angle method. DETAILED DESCRIPTION
[0018] Hereinafter, although the embodiment of the present invention is described by using the examples and comparative examples of the present invention based on the drawings, the present invention is not limited thereto and various forms are possible in the claims.
[0019] Figure 2 The manufacture of a glass particle deposit is schematically shown in FIG. The core deposition burner 13 is located at the bottom and is set independently of the cladding deposition burners 14 and 15 so that in addition to silicon tetrachloride, dopant raw materials such as germanium tetrachloride can be added at the same time. In most cases, multiple burners are configured in this way to manufacture gray particles. After the core is deposited on the starting material 11 using the core deposition burner 13, the cladding is deposited in a covering manner from the outside using the cladding deposition burners 14 and 15 arranged above the core deposition burner 13. [Example]
[0020] In Example 1 of the present embodiment, a glass particle deposit was produced under the following conditions using a total of three burners consisting of a core portion deposition burner 13, a first cladding portion deposition burner 14, and a second cladding portion deposition burner 15. Figure 3 The cross-sectional shapes of the first cladding portion deposition burner 14 and the second cladding portion deposition burner 15 are shown in FIG. The core portion deposition burner 13 uses a concentric quadruple tube burner, and silicon tetrachloride flows at 0.32 L / min, germanium tetrachloride flows at 15 mL / min, and argon as a carrier gas flows at 0.19 L / min through the central tube. Hydrogen flows at 6.2 L / min through the second tube from the center, argon as a sealing gas flows at 0.75 L / min through the third tube, and oxygen flows at 10.2 L / min through the outermost tube. Silicon tetrachloride flows at 0.80 L / min and oxygen flows at 0.66 L / min through the nozzle 21a of the first cladding portion deposition burner, hydrogen flows at 30 L / min through the nozzle 21d, oxygen flows at 18 L / min through the nozzle 21f, and a total of 1.5 L / min of oxygen flows through the small-diameter nozzle group 21c. On the other hand, silicon tetrachloride flows through the nozzle 21a of the burner for deposition of the second cladding portion at 4.8 L / min and oxygen flows through the nozzle 21a at 3.6 L / min, hydrogen flows through the nozzle 21d at 65 L / min, and oxygen flows through the nozzle 21f at 31 L / min. A total of 6.2 L / min of oxygen flows through the small-diameter nozzle group 21c.
[0021] The glass particle deposit obtained under such conditions is heated to about 1200°C in a furnace core tube containing chlorine gas for dehydration treatment, and then heated to about 1550°C in a furnace core tube containing helium gas for transparent vitrification to obtain a core glass rod.
[0022] The refractive index distribution of the core glass rod of Example 1 was measured by the refraction angle method, and the Figure 4 ,Should Figure 4 The relationship between the core radius position and the relative refractive index difference is shown. The optical properties are calculated by assuming that a cladding is added to a core glass rod with this refractive index distribution. Then, the cutoff wavelength of the optical fiber is actually measured after the cladding is actually added to the core glass rod and the fiber is drawn. The result shows that the deviation between the estimated cutoff wavelength calculated previously and the measured value is small, at 7nm.
[0023] use Figure 4 The numerical values of this embodiment are described below. When the relative refractive index difference ratio at the core center is set to 1.00, the position where the relative refractive index difference ratio is 0.45 is set to the core radius position r 0.45 , r 0.45 is 11.52mm. 0.45 There is a radius position r within the inner 5% range (0.576 mm) showing the maximum value ΔM of the relative refractive index difference. ΔM , ΔM=0.254%, r ΔM =11.47mm. Moreover, there is a minimum value of the relative refractive index difference Δm=0.216% on the inner side. The value of ΔM-Δm is 0.038%. In addition, the relative refractive index difference at the center, 0.75 times the radius position r 0.75 Located at the radius position r of the maximum value ΔM ΔM Further inward, radius position r 0.75 With r 0.45 R 0.75 / r 0.45 is 0.942. Thus, by 0.75 Set at more than r 0.45 5% of the inner side (i.e. r 0.75 / r 0.45 <0.95), the wavelength dispersion of the obtained optical fiber at a wavelength of 1550nm can be designed to be smaller.
[0024] In Examples 2 to 5, core glass rods were produced in the same manner as in Example 1, and the ΔM-Δm (%) value of the core glass rods and the degree of deviation between the estimated cutoff wavelength and the measured optical fiber cutoff wavelength were determined. The results are summarized in Table 1.
[0025] In Example 6 of the present embodiment, a glass particle deposit was produced under the following conditions using a total of three burners consisting of a core deposition burner 13, a first cladding deposition burner 14, and a second cladding deposition burner 15. The core deposition burner 13 used a concentric quadruple tube burner, and silicon tetrachloride flowed through the center tube at 0.30 L / min, germanium tetrachloride flowed through the center tube at 15 mL / min, and argon flowed through the center tube at 0.19 L / min as a carrier gas. Hydrogen flowed through the second tube from the center at 5.8 L / min, argon flowed through the third tube as a sealing gas at 1.3 L / min, and oxygen flowed through the outermost tube at 9.5 L / min. The first cladding deposition burner 14 used a concentric quadruple tube burner, and silicon tetrachloride flowed through the center tube at 0.96 L / min, and argon flowed through the center tube at 0.90 L / min as a carrier gas. Hydrogen flows through the second tube from the center at 16.7 L / min, argon as a sealing gas flows through the third tube at 1.50 L / min, and oxygen flows through the outermost tube at 15.1 L / min. On the other hand, the burner 15 for the second cladding deposition adopts a concentric quintuple tube burner, silicon tetrachloride flows through the center tube at 3.5 L / min, and oxygen flows through the center tube at 2.8 L / min. Nitrogen flows through the second tube from the center at 2.2 L / min, hydrogen flows through the third tube at 60 L / min, nitrogen flows through the fourth tube at 3.0 L / min, and oxygen flows through the outermost tube at 40 L / min.
[0026] The glass particle deposit obtained under such conditions is heated to about 1100°C in a furnace core tube containing chlorine gas for dehydration treatment, and then heated to about 1500°C in a furnace core tube containing helium gas for transparent vitrification to obtain a core glass rod.
[0027] The refractive index distribution of the core glass rod of Example 6 was measured by the refraction angle method, and the Figure 5 ,Should Figure 5 The relationship between the core radius position and the relative refractive index difference is shown. Compared with Example 1, the flow rate of silicon tetrachloride in the glass raw material supplied to the burner for core deposition is reduced, so the core radius r 0.45 Slightly thinner than Example 1, 10.0 mm. 0.45 There is a radius position r within the inner 5% range (0.500 mm) showing the maximum value ΔM of the relative refractive index difference. ΔM , ΔM=0.320%, r ΔM =9.724 mm. Moreover, there is a minimum value of the relative refractive index difference Δm=0.308% on the inner side. The value of ΔM-Δm is 0.012%. In addition, since the temperature of the dehydration treatment is set lower than that of Example 1, the radial position r 0.75 With r 0.45 R0.75 / r 0.45 is 0.984. Thus, by changing the radius position r 0.75 Set at ratio r ΔM More outboard (ie r 0.75 <r ΔM ), the zero dispersion wavelength of the obtained optical fiber can be designed to be smaller. It is assumed that a cladding is added to a core glass rod having such a refractive index distribution and the optical characteristics are estimated. In addition, the cutoff wavelength of the optical fiber is actually measured after the cladding is actually added to the core glass rod and the fiber is drawn. As a result, the deviation between the estimated value of the cutoff wavelength calculated previously and the measured value is small, which is 5nm. [Comparative Example]
[0028] In Comparative Example 1 of the present embodiment, a glass particle deposit was produced under the following conditions using a total of three burners consisting of a core portion deposition burner 13, a first cladding portion deposition burner 14, and a second cladding portion deposition burner 15. Figure 3 The cross-sectional shapes of the first cladding portion deposition burner 14 and the second cladding portion deposition burner 15 are shown in FIG. The core portion deposition burner 13 uses a concentric quadruple tube burner, and silicon tetrachloride flows at 0.36 L / min, germanium tetrachloride flows at 16 mL / min, and argon as a carrier gas flows at 0.19 L / min through the central tube. Hydrogen flows at 6.5 L / min through the second tube from the center, argon as a sealing gas flows at 0.75 L / min through the third tube, and oxygen flows at 10.2 L / min through the outermost tube. Silicon tetrachloride flows at 0.80 L / min and oxygen flows at 0.66 L / min through the nozzle 21a of the first cladding portion deposition burner, hydrogen flows at 34 L / min through the nozzle 21d, oxygen flows at 18 L / min through the nozzle 21f, and a total of 1.5 L / min of oxygen flows through the small-diameter nozzle group 21c. On the other hand, silicon tetrachloride flows at 4.8 L / min and oxygen flows at 3.6 L / min through the nozzle 21a of the burner for deposition of the second cladding portion, hydrogen flows at 65 L / min through the nozzle 21d, and oxygen flows at 31 L / min through the nozzle 21f. A total of 6.2 L / min of oxygen flows through the small-diameter nozzle group 21c.
[0029] The prepared glass particle deposit is heated to about 1200°C in a furnace core tube containing chlorine gas for dehydration treatment, and then heated to about 1550°C in a furnace core tube containing helium gas for transparent vitrification to obtain a core glass rod.
[0030] The refractive index distribution of the core glass rod of Comparative Example 1 was measured by the refraction angle method, and the Figure 6The optical properties were estimated by assuming that a cladding was added to a core glass rod with this refractive index distribution. Then, the cutoff wavelength of the optical fiber was actually measured after the cladding was actually added to the core glass rod and the fiber was drawn. The measured cutoff wavelength was significantly larger than the estimated value, deviating by 67nm.
[0031] according to Figure 6 When the ratio of the relative refractive index difference at the core center is set to 1.00, the position where the relative refractive index difference ratio is 0.45 is set as the core radius position. Within the 5% range inside (0.581mm inside and outside), there is a maximum value of the relative refractive index difference ΔM=0.272%, and outside it, there is a minimum value of the relative refractive index difference Δm=0.193%. The value of ΔM-Δm is 0.079%, and the estimated cut-off wavelength deviates significantly from the measured fiber cut-off wavelength.
[0032] In Comparative Examples 2 to 5, core glass rods were produced in the same manner as in Comparative Example 1, and the ΔM-Δm (%) values of the core glass rods and the degree of deviation between the estimated cutoff wavelength and the measured optical fiber cutoff wavelength were determined. The results are summarized in Table 1.
[0033] In Table 1, the values of ΔM-Δm (%) of Examples 1 to 5 are small, all below 0.04%, and the deviation between the estimated cutoff wavelength (nm) and the measured optical fiber cutoff wavelength (nm) is also small, below 10nm, and it can be said that the estimation accuracy of the cutoff wavelength is good. In contrast, the values of ΔM-Δm (%) of Comparative Examples 1 to 5 exceed 0.04%, and the deviation between the estimated cutoff wavelength (nm) and the measured optical fiber cutoff wavelength (nm) is also far more than 10nm. [Table 1] [Explanation of Reference Numerals]
[0034] 11: Starting Materials 12: Glass particle deposit 13: Burner for core deposition 14: Burner for the first cladding deposition 15: Burner for second cladding deposition 20: Burner 21a: Innermost gas outlet 21b: The second gas outlet from the inside 21c: The small-diameter nozzle group in the third gas outlet area from the inside 21d: The third gas outlet from the innermost 21e: the fourth gas outlet from the inside 21f: the fifth gas outlet from the inside.
Claims
1. An optical fiber mother material, characterized in that: When manufacturing a core glass matrix composed of a core portion and a portion of a cladding portion, and then providing the remaining cladding portion to the outside of the core glass matrix, in the core glass matrix, a radius position at which the relative refractive index difference is 0.45 times the relative refractive index difference at the core center is set as the core radius position, and within 5% inside the core radius position, there are a point with a maximum value ΔM indicating a locally high relative refractive index difference and a point with a minimum value Δm indicating a locally low relative refractive index difference, and the value of ΔM-Δm does not exceed 0.04%.
2. The optical fiber mother material according to claim 1, characterized in that: The value of ΔM-Δm does not exceed 0.03%.
3. The optical fiber mother material according to claim 1, characterized in that: The value of ΔM-Δm does not exceed 0.02%.
4. The optical fiber mother material according to claim 1, characterized in that: The value of ΔM-Δm does not exceed 0.01%.
5. A method for manufacturing an optical fiber mother material, characterized in that: The invention relates to a method for manufacturing an optical fiber mother material, in which a core glass mother material consisting of a core part and a part of a cladding part is manufactured, and then the remaining cladding part is provided to the outside of the core glass mother material; in the core glass mother material, a radius position at which the relative refractive index difference is 0.45 times the relative refractive index difference at the core center is set as the core radius position, and within 5% of the inner side of the core radius position, there are a point having a maximum value ΔM indicating a locally high relative refractive index difference and a point having a minimum value Δm indicating a locally low relative refractive index difference, and the remaining cladding part is provided to the outside of the core glass mother material whose value of ΔM-Δm does not exceed 0.04%.
6. The method for manufacturing an optical fiber mother material according to claim 5, characterized in that: The value of ΔM-Δm does not exceed 0.03%.
7. The method for manufacturing an optical fiber mother material according to claim 5, characterized in that: The value of ΔM-Δm does not exceed 0.02%.
8. The method for manufacturing an optical fiber mother material according to claim 5, characterized in that: The value of ΔM-Δm does not exceed 0.01%.