Substrate processing method, semiconductor device manufacturing method, substrate processing apparatus, and program
By alternating the use of raw material gas and crystal growth inhibitor gas in the substrate, the formation process of multilayer films is controlled, solving the problem of film quality deterioration caused by excessive residual stress, and achieving improvement in film quality and productivity.
Patent Information
- Application Number
- CN202380034652.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-26
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-26
AI Technical Summary
When polycrystalline films are formed on a substrate, excessive residual stress in the film leads to film degradation.
By alternating the circulation of raw material gas and crystal growth inhibitor gas on the substrate, the formation process of multilayer films is controlled, ensuring that the absolute value and gradient of residual stress in the multilayer films are less than the allowable values.
It improves the film quality formed on the substrate, controls the residual stress of multilayer films, reduces warpage, enhances the uniformity of film crystal size and surface roughness, and improves productivity.
Smart Images

Figure CN119032197A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a substrate processing method, a method for manufacturing a semiconductor device, a substrate processing apparatus, and a program. Background Art
[0002] As one of the steps in the process of manufacturing a semiconductor device, a process of forming a polycrystalline film on a substrate is sometimes performed (for example, refer to Patent Documents 1 to 7).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-43262
[0006] Patent Document 2: Japanese Patent Application Publication No. 2016-1760
[0007] Patent Document 3: Japanese Patent Application Publication No. 2009-81457
[0008] Patent Document 4: Japanese Patent Application Publication No. 2013-197307
[0009] Patent Document 5: Japanese Patent Application Publication No. 2009-147388
[0010] Patent Document 6: Japanese Patent Application Publication No. 2018-160516
[0011] Patent Document 7: International Publication No. 2022 / 064578 Pamphlet Summary of the invention
[0012] Problems to be solved by the invention
[0013] When a polycrystalline film is formed on a substrate, residual stress in the film increases, which may cause degradation in the film quality of the film formed on the substrate.
[0014] The present disclosure provides a technology capable of improving the film quality of a film formed on a substrate.
[0015] Methods used to solve problems
[0016] According to one embodiment of the present disclosure, a technology is provided, which comprises a process of forming a multilayer film of a specified thickness on a substrate by performing a cycle including (a) and (b) a specified number of times, wherein (a) is a process of depositing an initial film by exposing the substrate to a raw material gas; and (b) is a process of exposing the substrate to a crystal growth inhibiting gas or a specified gas for forming a film having a different film quality from the initial film, and the specified number of times is set so that after annealing the multilayer film, the absolute value or gradient of the residual stress of the multilayer film is less than an allowable value.
[0017] Effects of the Invention
[0018] According to the present disclosure, the film quality of a film formed on a substrate can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic structural diagram of a vertical processing furnace of a substrate processing apparatus that can be suitably used in one embodiment of the present disclosure, and is a diagram showing a processing furnace 202 portion in a vertical cross-sectional view.
[0020] Figure 2 It is a schematic configuration diagram of a controller 121 of a substrate processing apparatus that can be suitably used in one embodiment of the present disclosure, and is a diagram showing a control system of the controller 121 in a block diagram.
[0021] Figure 3 This is a diagram showing a flow chart in a substrate processing step according to one embodiment of the present disclosure.
[0022] Figure 4 (A) is a diagram showing the cross-section of the substrate of samples 1 and 2 formed by the substrate processing step of the comparative example, Figure 4 (B) in FIG. 1 is a diagram showing a cross section of the substrate of samples 3 and 4 formed by the substrate processing step of this example.
[0023] Figure 5 It is a diagram showing a processing sequence in a film forming step according to one embodiment of the present disclosure.
[0024] Figure 6 This is a diagram showing the results of SIMS analysis of oxygen in a film of a substrate after a substrate treatment step according to one embodiment of the present disclosure.
[0025] Figure 7 It is a diagram showing the measurement results of the residual stress of a film formed on a substrate in the case where there is no annealing step and in the case where there is an annealing step in the substrate processing step according to one embodiment of the present disclosure.
[0026] Figure 8 (A) is a diagram showing the cross-section of the substrate of samples 1 and 2 formed by the substrate processing step of the comparative example, Figure 8 (B) in FIG. 1 is a diagram showing a cross section of the substrate of samples 3 and 4 formed by the substrate processing step of this example.
[0027] Fig. 9 (A) in FIG. 1 is a diagram showing a cross-sectional TEM image of sample 1 in Experiment 3. FIG. Fig. 9 (B) in FIG. 3 is a diagram showing a cross-sectional TEM image of sample 3 of experiment 3.
[0028] Fig.10(A) in FIG. 3 is a diagram showing a cross-sectional TEM image of sample 2 in Experiment 3. FIG. Fig.10 (B) in FIG. 3 is a diagram showing a cross-sectional TEM image of sample 4 of Experiment 3. FIG.
[0029] Fig.11 (A) in FIG. 3 is a diagram showing the results of XRD analysis of the film on the substrate of Sample 2 in Experiment 3. FIG. Fig.11 (B) in FIG. 3 is a diagram showing the results of XRD analysis of the film on the substrate of Sample 4 in Experiment 3.
[0030] Fig.12 (A) is a diagram showing a cross-sectional SEM image of sample 2 of Experiment 4. Fig.12 (B) in FIG. 4 is a diagram showing a cross-sectional SEM image of sample 4 of experiment 4.
[0031] Fig.13 (A) in FIG. 1 is a diagram showing the range of the cross-sectional EBSD analysis of Sample 2 of Experiment 4 in the cross-sectional TEM image. Fig.13 (B) in FIG. 4 is a diagram showing the range of the cross-sectional EBSD analysis of Sample 4 of Experiment 4 in the cross-sectional TEM image.
[0032] Fig.14 This is the anti-pole diagram orientation map of samples 2 and 4 of experiment 4 obtained by cross-section EBSD.
[0033] Figure 15 is the anti-pole diagram image of samples 2 and 4 in Experiment 4.
[0034] Fig.16 (A) is a SEM image of the cantilever produced by sample 2 of experiment 4. Fig.16 (B) is a SEM image of the cantilever produced by sample 4 of experiment 4.
[0035] Fig.17 Graphs showing contour curves of displacement amounts on the surfaces of the cantilevers of samples 2 and 4 of Experiment 4. DETAILED DESCRIPTION
[0036] <One aspect of the present disclosure>
[0037] Below, mainly refer to Figure 1 to Figure 5 , while explaining one mode of the present disclosure. In addition, the drawings used in the following description are all schematic drawings, and the relationship between the dimensions of the elements and the proportions of the elements shown in the drawings are not necessarily consistent with reality. In addition, the relationship between the dimensions of the elements and the proportions of the elements are not necessarily consistent between multiple drawings.
[0038] (1) Structure of substrate processing apparatus
[0039] like Figure 1As shown in FIG. 2 , the processing furnace 202 has a heater 207 as a temperature regulator (heating unit). The heater 207 is cylindrical and is vertically installed by being supported by a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) the gas by heat.
[0040] A reaction tube 203 is disposed inside the heater 207 and concentrically with the heater 207. The reaction tube 203 is made of, for example, quartz (SiO 2 ) or a heat-resistant material such as silicon carbide (SiC), and is formed into a cylindrical shape with an upper end blocked and a lower end open. A manifold 209 is arranged below the reaction tube 203. The manifold 209 is formed of a metal material such as stainless steel (SUS), and is formed into a cylindrical shape with an upper end and a lower end open. The upper end of the manifold 209 is engaged with the lower end of the reaction tube 203, and is configured to support the reaction tube 203. An O-ring 220a as a sealing component is provided between the manifold 209 and the reaction tube 203. The reaction tube 203 is installed vertically in the same manner as the heater 207. The processing container (reaction container) is mainly composed of the reaction tube 203 and the manifold 209. A processing chamber 201 is formed in the hollow portion of the processing container. The processing chamber 201 is configured to accommodate a wafer 200 as a substrate. The processing of the wafer 200 is performed in the processing chamber 201.
[0041] In the processing chamber 201, nozzles 249a to 249c as the first to third supply parts are respectively provided in a manner penetrating the side wall of the manifold 209. The nozzles 249a to 249c are also referred to as the first to third nozzles, respectively. The nozzles 249a to 249c are made of heat-resistant materials such as quartz, for example. Gas supply pipes 232a to 232c are respectively connected to the nozzles 249a to 249c. The nozzles 249a to 249c are nozzles of different lengths.
[0042] The nozzle 249a is arranged at a position above the wafer arrangement area extending from the lowermost wafer 200 to the uppermost wafer 200 along the wafer arrangement direction in the processing chamber 201. The nozzle 249c is arranged at a position below the wafer arrangement area extending along the wafer arrangement direction. The nozzle 249b is arranged at a position extending to the vicinity of the center of the wafer arrangement area. The nozzles 249a and 249c are arranged adjacent to the nozzle 249b, respectively. Gas supply holes 250a to 250c for supplying gas are respectively provided at the front ends of the nozzles 249a to 249c.
[0043] In the gas supply pipes 232a to 232c, mass flow controllers (MFC) 241a to 241c as flow controllers (flow control units) and valves 243a to 243c as opening and closing valves are provided in order from the upstream side of the gas flow. On the downstream side of the gas supply pipe 232a from the valve 243a, gas supply pipes 232d and 232e are connected respectively. On the downstream side of the gas supply pipe 232b from the valve 243b, gas supply pipes 232f and 232h are connected respectively. On the downstream side of the gas supply pipe 232c from the valve 243c, a gas supply pipe 232g is connected. In the gas supply pipes 232d to 232h, MFCs 241d to 241h and valves 243d to 243h are provided in order from the upstream side of the gas flow. The gas supply pipes 232a to 232h are made of metal materials such as SUS, for example.
[0044] The source gas is supplied from the gas supply pipes 232a to 232c through the MFCs 241a to 241c, valves 243a to 243c, and nozzles 249a to 249c into the processing chamber 201. The source gas may also be referred to as a first element-containing gas containing the first element as a source material.
[0045] The cleaning gas is supplied from the gas supply pipe 232 d into the processing chamber 201 via the MFC 241 d , the valve 243 d , and the nozzle 249 a .
[0046] The inert gas is supplied from the gas supply pipes 232e to 232g into the processing chamber 201 via the MFCs 241e to 241g, the valves 243e to 243g, the gas supply pipes 232a to 232c, and the nozzles 249a to 249c, respectively.
[0047] The crystal growth inhibiting gas that affects the crystal growth of the source gas is supplied from the gas supply pipe 232h into the processing chamber 201 via the MFC 241h, the valve 243h, the gas supply pipe 232b, and the nozzle 249b.
[0048] The raw material gas supply system (also called the film forming gas supply system) is mainly composed of the gas supply pipes 232a to 232c, MFC241a to 241c, and valves 243a to 243c. The cleaning gas supply system is mainly composed of the gas supply pipes 232d, MFC241d, and valve 243d. The inert gas supply system is mainly composed of the gas supply pipes 232e to 232g, MFC241e to 241g, and valves 243e to 243g. The crystal growth hindering gas supply system is mainly composed of the gas supply pipe 232h, MFC241h, and valve 243h.
[0049] Here, since the raw material gas functions as a film-forming gas or a gas containing the first element, the raw material gas supply system can also be referred to as a film-forming gas supply system or a gas supply system containing the first element.
[0050] One or all of the various supply systems described above may be configured as an integrated supply system 248 that integrates valves 243a to 243h and MFCs 241a to 241h. The integrated supply system 248 is connected to the gas supply pipes 232a to 232h, respectively, and is configured to control the supply operation of various gases in the gas supply pipes 232a to 232h, that is, the opening and closing operation of the valves 243a to 243h and the flow rate adjustment operation performed by the MFCs 241a to 241h, etc., through the controller 121 described later. The integrated supply system 248 is configured as an integrated unit of an integral type or a split type, and can be loaded and unloaded relative to the gas supply pipes 232a to 232h, etc., as an integrated unit, and is configured to be able to be repaired, replaced, and added as an integrated unit.
[0051] An exhaust port 231a for exhausting the gas atmosphere in the processing chamber 201 is provided below the side wall of the reaction tube 203. The exhaust port 231a can be provided at a position opposite to (opposite to) the nozzles 249a to 249c (gas supply holes 250a to 250c) in a manner of sandwiching the wafer 200. The exhaust port 231a can be provided on the side wall of the manifold 209, or can be provided from the lower part of the side wall of the reaction tube 203 along the upper part, that is, along the wafer arrangement area. An exhaust pipe 231 is connected to the exhaust port 231a. A vacuum pump 246 as an exhaust device is connected to the exhaust pipe 231 via a pressure sensor 245 as a pressure detector (pressure detection unit) that detects the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure regulating unit). The APC valve 244 is configured to open and close the valve while the vacuum pump 246 is in operation, thereby enabling vacuum exhaust and vacuum exhaust stop in the processing chamber 201. Furthermore, the valve opening is adjusted based on pressure information detected by the pressure sensor 245 while the vacuum pump 246 is in operation, thereby enabling the pressure in the processing chamber 201 to be adjusted. The exhaust system is mainly composed of the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. It is also conceivable that the vacuum pump 246 is included in the exhaust system.
[0052] A sealing cap 219 as a furnace cover capable of hermetically closing the lower end opening of the manifold 209 is provided below the manifold 209. The sealing cap 219 is made of a metal material such as SUS and is formed into a disc shape. An O-ring 220b as a sealing member abutting against the lower end of the manifold 209 is provided on the upper surface of the sealing cap 219. A rotating mechanism 267 for rotating the wafer boat 217 described later is provided below the sealing cap 219. The rotating shaft 255 of the rotating mechanism 267 passes through the sealing cap 219 and is connected to the wafer boat 217. The rotating mechanism 267 is configured to rotate the wafer 200 by rotating the wafer boat 217. The sealing cap 219 is configured to be lifted and lowered in the vertical direction by the wafer boat lifter 115 as a lifting mechanism provided outside the reaction tube 203. The boat elevator 115 is configured as a transport device (transport mechanism) that carries the wafer 200 into and out of the processing chamber 201 (transports) by raising and lowering the sealing cap 219 .
[0053] A gate 219s as a furnace cover is provided below the manifold 209 so as to close the lower end opening of the manifold 209 when the sealing cap 219 is lowered and the wafer boat 217 is carried out from the processing chamber 201. The gate 219s is formed into a disc shape using a metal material such as SUS. An O-ring 220c as a sealing member that abuts against the lower end of the manifold 209 may be provided on the top of the gate 219s. The opening and closing actions (lifting and rotating actions, etc.) of the gate 219s are controlled by the gate opening and closing mechanism 115s.
[0054] The wafer boat 217 as a substrate support is configured to support multiple wafers 200, for example, 25 to 200 wafers, in a horizontal position and with their centers aligned with each other in a vertical direction, and to support them in multiple layers, that is, to support them in a spaced manner. The wafer boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the wafer boat 217, a heat shield 218 is supported in multiple layers.
[0055] A temperature sensor 263 as a temperature detector is provided in the reaction tube 203. The degree of power supplied to the heater 207 is adjusted based on the temperature information detected by the temperature sensor 263, so that the temperature in the processing chamber 201 has a desired temperature distribution. The temperature sensor 263 is provided along the inner wall of the reaction tube 203.
[0056] like Figure 2As shown, the controller 121 as a control unit (control unit) is configured as a computer having a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. The controller 121 is connected to an input / output device 122 configured as a touch panel, etc.
[0057] The storage device 121c is composed of, for example, a flash memory, a HDD (Hard Disk Drive), an SSD (Solid State Drive), etc. A control program for controlling the operation of the substrate processing device, and a process recipe described later that records the process and conditions of the substrate processing, etc. are readable and stored in the storage device 121c. The process recipe is combined in a manner that enables the controller 121 to execute each process in the substrate processing described later and to obtain a specified result, and functions as a program. Hereinafter, process recipes and control programs are also simply referred to as programs. In addition, process recipes are also simply referred to as recipes. When the term "program" is used in this specification, there is a case where only a recipe is included, a case where only a control program is included, or a case where both are included. RAM121b is configured as a memory area (working area) that temporarily holds programs or data read out by CPU121a.
[0058] The I / O port 121d is connected to the above-mentioned MFCs 241a to 241h, valves 243a to 243h, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotation mechanism 267, boat elevator 115, gate opening and closing mechanism 115s, etc.
[0059] The CPU 121a is configured to read out and execute a control program from the storage device 121c, and to read out a recipe from the storage device 121c in accordance with input of an operation command from the input / output device 122. The CPU 121a is configured to control, according to the contents of the read recipe, flow rate adjustment operations of various gases by the MFCs 241a to 241h, opening and closing operations of the valves 243a to 243h, opening and closing operations of the APC valve 244, and pressure adjustment operations by the APC valve 244 based on the pressure sensor 245, start and stop of the vacuum pump 246, temperature adjustment operations of the heater 207 based on the temperature sensor 263, rotation of the wafer boat 217 and rotation speed adjustment operations by the rotation mechanism 267, lifting and lowering operations of the wafer boat 217 by the wafer boat lifter 115, and opening and closing operations of the gate 219s by the gate opening and closing mechanism 115s.
[0060] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 into the computer. The external storage device 123 includes, for example, a disk such as an HDD, an optical disk such as a CD, an optical disk such as an MO, a USB memory, a semiconductor memory such as an SSD, etc. The storage device 121c or the external storage device 123 is configured as a computer-readable recording medium. Hereinafter, they are also simply collectively referred to as recording media. In addition, the program can be provided to the computer without using the external storage device 123, but using a communication unit such as the Internet or a dedicated line.
[0061] (2) Substrate processing steps
[0062] Using the above-mentioned substrate processing apparatus, as one step of the manufacturing process of a semiconductor device (module), a processing sequence example of forming a film on the surface of a wafer 200 is mainly used. Figure 3 , Figure 4 (B) and Figure 5 Here, a sacrificial layer 300 is previously formed on the surface of the wafer 200 . In the following description, the operations of the various components constituting the substrate processing apparatus are controlled by the controller 121 .
[0063] When the term "wafer" is used in this specification, there are cases where it refers to the wafer itself and cases where it refers to a stack of a wafer and a predetermined layer or film formed on its surface. When the term "surface of the wafer" is used in this specification, there are cases where it refers to the surface of the wafer itself and cases where it refers to the surface of a predetermined layer, etc. formed on the wafer. When it is recorded in this specification as "a predetermined layer is formed on the wafer", there are cases where it refers to directly forming a predetermined layer on the surface of the wafer itself and cases where it refers to forming a predetermined layer above a layer, etc. formed on the wafer. When the term "substrate" is used in this specification, it is synonymous with the use of the term "wafer".
[0064] [Film Forming Step S110]
[0065] First, in the film forming step S110, use Figure 4 (B) and Figure 5 To explain.
[0066] Here, a source gas and a crystal growth inhibiting gas are used and these gases are alternately supplied to form a multi-layer film on the surface of the sacrificial layer 300 of the wafer 200 .
[0067] That is, the film forming process includes step C of forming a multilayer film of a specified thickness on the wafer 200 by performing a cycle including step A and step B for a specified number of times (n times, n is an integer greater than 1), wherein step A refers to depositing a polycrystalline film as an initial film (primitive film) by exposing the wafer 200 to a raw material gas; and step B refers to exposing the wafer 200 to a crystal growth inhibiting gas, and the specified number of times is set so that after annealing the multilayer film, the absolute value or gradient of the residual stress of the multilayer film is less than an allowable value.
[0068] In the above-mentioned film forming process, step B is performed under the condition that the polycrystalline film deposited in the subsequent step A forms new crystal grains.
[0069] In this specification, the above-mentioned processing sequence is also shown as follows for the convenience of description. The same expression is also used in the description of other aspects, modified examples, etc. below.
[0070] (raw material gas → crystal growth inhibiting gas) × n
[0071] (Wafer filling and wafer boat loading)
[0072] When a plurality of wafers 200 are loaded into the wafer boat 217 (wafer filling), the gate 219s is moved by the gate opening and closing mechanism 115s, and the lower end opening of the manifold 209 is opened (gate opening). Figure 1 As shown, the wafer boat 217 supporting the plurality of wafers 200 is lifted by the wafer boat lifter 115 and carried into (wafer boat loading) the processing chamber 201, and finally the processing chamber 201 is airtightly closed by the sealing cap 219. At this time, an inert gas is supplied into the processing chamber 201, and the temperature in the processing chamber 201 is maintained at a desired temperature.
[0073] (Vacuum exhaust and temperature adjustment)
[0074] After that, vacuum exhaust (decompression exhaust) is performed by the vacuum pump 246 in such a manner that the processing chamber 201, that is, the space where the wafer 200 is located, is brought to a desired pressure (vacuum degree). At this time, the pressure in the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information. In addition, the heater 207 is used to heat the wafer 200 in the processing chamber 201 so that it reaches a desired processing temperature. At this time, the degree of power supply to the heater 207 is feedback-controlled based on the temperature information detected by the temperature sensor 263 so that the processing chamber 201 has a desired temperature distribution. In addition, the rotation of the wafer 200 by the rotation mechanism 267 is started. The exhaust in the processing chamber 201, the heating and rotation of the wafer 200 are all continuously performed at least until the processing of the wafer 200 is completed.
[0075] After that, step A and step B are executed in this order. Hereinafter, each of these steps will be described.
[0076] [Step A]
[0077] In step A, raw material gas is supplied to the wafer 200 in the processing chamber 201, and a polycrystalline film is deposited (film formed) on the surface of the wafer 200 by exposing the wafer 200 to the raw material gas. Thereafter, the supply of the raw material gas is stopped, and the raw material gas remaining in the processing chamber 201 is exhausted (purged).
[0078] Specifically, valves 243a to 243c are opened, and the raw material gas is supplied to the gas supply pipes 232a to 232c. The raw material gas is flow-regulated by MFCs 241a to 241c, and supplied to the processing chamber 201 through nozzles 249a to 249c, and exhausted from the exhaust port 231a. At this time, the raw material gas system is supplied to the wafer 200 and exposed to the raw material gas. At this time, the pressure in the processing chamber 201 is maintained at a predetermined processing pressure by the APC valve 244.
[0079] By supplying raw material gas (also referred to as exposure) to the wafer 200 under the processing conditions described later, the initial film is deposited on the surface of the wafer 200 by the thermal CVD method and a polycrystalline film 400 is formed. The polycrystalline film 400 is, for example, a film containing a Group 14 element. In the present embodiment, since a batch processing chamber with a hot wall type is used, most of the CVD will be accompanied by a gas phase reaction, in contrast to a cold wall type processing chamber in which a surface reaction is the main body. The film quality of the film obtained by various types of processing chambers may be different. For example, compared with the Epi-poly Si film manufactured by a cold wall type single-chip device, the poly-Si film manufactured by a hot wall type reduced pressure CVD device has a tendency to have a greater compressive stress or stress gradient. The reaction intermediates supplied by the gas phase reaction are helpful for forming a high-quality film at a low temperature, but they will produce the residual atoms described later and may cause an increase in residual stress.
[0080] The raw material gas is a gas for depositing the polycrystalline film 400 on the wafer 200, and is, for example, a gas containing a Group 14 element, such as a Si-containing gas containing silicon (Si). The Si-containing gas may be, for example, a gas containing monosilane (SiH 4 ) gas. 4 When the raw material gas is SiH 4 The gas is thermally decomposed to form a polycrystalline silicon film as a polycrystalline film on the surface of the wafer 200. The raw material gas may contain hydrogen (H 2 ) gas or nitrogen (N 2 ) gas, helium (He) gas, argon (Ar) gas and other reducing gases or carrier gases, diluent gases.
[0081] Examples of the processing conditions when the raw material gas is supplied in step A include:
[0082] Processing temperature: 400-1090°C, preferably 500-750°C;
[0083] Processing pressure: 1-100000Pa, preferably 10-1000Pa;
[0084] Raw material gas supply flow rate: 10 to 5000 sccm, preferably 100 to 1500 sccm;
[0085] Film forming speed: 0.1-30 nm / min, preferably 1-20 nm / min;
[0086] Inert gas supply flow rate (per gas supply pipe): 0 to 3000 sccm.
[0087] At the end of step A, the valves 243a to 243c are closed to stop the supply of the raw material gas, and the processing chamber 201 is evacuated to remove the raw material gas and the like remaining in the processing chamber 201 from the processing chamber 201. At this time, an inert gas is supplied to the processing chamber 201 through the nozzles 249a to 249c. The inert gas supplied through the nozzles 249a to 249c acts as a purge gas, and thus the processing chamber 201 is purged.
[0088] As the inert gas, for example, N 2 As the gas, other rare gases such as Ar gas, He gas, neon (Ne) gas, and xenon (Xe) gas may be used. This also applies to each step described later.
[0089] Examples of the treatment conditions for purging in step A include:
[0090] Processing temperature: 400-1090°C, preferably the same temperature as when the raw material gas is supplied;
[0091] Processing pressure: 1-5000Pa, preferably 5-1000Pa;
[0092] Inert gas supply flow rate (each gas supply pipe): 0.1~5000sccm;
[0093] Inert gas supply time: 1 to 3000 seconds.
[0094] In addition, the expression of a numerical range such as "1000-100000Pa" in this specification means that the lower limit and the upper limit are included in the range. Therefore, for example, "1000-100000Pa" means "above 1000Pa and below 100000Pa". The same is true for other numerical ranges. In addition, the processing temperature in this specification refers to the temperature of the wafer 200 or the temperature in the processing chamber 201, and the processing pressure refers to the pressure in the processing chamber 201. In addition, the processing time refers to the time during which the processing continues. These are also the same in the following descriptions.
[0095] [Step B]
[0096] After step A is completed, step B is performed. In step B, a crystal growth inhibiting gas and an inert gas are supplied to the wafer 200 in the processing chamber 201. That is, the wafer 200 after the polycrystalline film 400 is formed on the surface is exposed to the crystal growth inhibiting gas. Thus, a crystal growth inhibiting layer (also referred to as a crystal growth inhibiting film) 500 is formed on the surface of the wafer 200 on which the polycrystalline film is formed. Then, the supply of the crystal growth inhibiting gas and the inert gas is stopped, and the gas remaining in the processing chamber 201 is exhausted.
[0097] Specifically, valve 243h is opened, and crystal growth inhibiting gas is supplied to gas supply pipe 232b. Crystal growth inhibiting gas is adjusted in flow rate by MFC241h, supplied to processing chamber 201 via nozzle 249b, and exhausted from exhaust port 231a. At this time, crystal growth inhibiting gas is supplied to wafer 200 having a polycrystalline film formed on the surface and is exposed to the crystal growth inhibiting gas. At this time, inert gas is supplied to processing chamber 201 via nozzles 249a to 249c respectively while valves 243e to 243g are opened.
[0098] By supplying a crystal growth inhibiting gas to the wafer 200 under the processing conditions described later and exposing the wafer 200 to the crystal growth inhibiting gas, a layer including elements other than the elements constituting the polycrystalline film, i.e., a crystal growth inhibiting layer 500, is formed on the surface of the polycrystalline film formed in the immediately preceding step A. The crystal growth inhibiting layer 500 stops the continuous crystal growth of microcrystals (crystal grains) constituting the polycrystalline film.
[0099] Step B is performed under the condition that the polycrystalline film deposited in the subsequent step A described later forms new crystal grains. That is, by exposing the wafer 200 having a polycrystalline film formed on the surface to a crystal growth inhibiting gas, the polycrystalline film deposited in the subsequent step A can form new crystal grains. In other words, with step B as an opportunity, the grain boundaries of the polycrystalline film formed on the surface of the wafer 200 are capped, and the polycrystalline film deposited in the subsequent step A is given crystal nuclei at a predetermined density, and crystals that are discontinuous with the crystals of the substrate are grown. The crystal growth inhibiting layer 500 is not limited to being formed during step B, and may also include an amorphous or other low-crystallinity layer formed in the initial stage of the subsequent step A.
[0100] The thickness of the film or layer formed in step B is thinner than the thickness of the polycrystalline film formed in the immediately preceding step A, for example, less than 1 / 10 of the thickness of the polycrystalline film formed in the immediately preceding step A. Alternatively, step B may modify or remove a portion of the film formed in the immediately preceding step A, or change (reconstruct) the surface state.
[0101] Next, the valve 243h and valves 243e to 243g are closed to stop the supply of the crystal growth inhibiting gas and the inert gas, and the processing chamber 201 is evacuated to remove the gas remaining in the processing chamber 201 .
[0102] As the processing conditions when the crystal growth inhibiting gas is supplied in step B, there are exemplified:
[0103] Processing pressure: 1-10000Pa, preferably 1-1000Pa;
[0104] Crystal growth hindering gas supply flow rate: 0.1 to 5000 sccm, preferably 10 to 500 sccm;
[0105] Crystal growth hindering gas supply time: 0.1 second to 30 minutes;
[0106] Preferably, it is 1 second to 3 minutes; inert gas supply flow rate (for each gas supply pipe): 0 to 3000 sccm.
[0107] As the processing conditions when exhausting in step B, there are exemplified:
[0108] Processing pressure: 0.1-5000Pa, preferably 10-1000Pa.
[0109] In addition, in step B, the output of the heater 207 is adjusted so that the processing temperature is the same as the processing temperature in step A.
[0110] As the crystal growth inhibiting gas, for example, a gas containing oxygen (O) or a gas containing nitrogen (N) can be used. As the O-containing gas, for example, an oxygen (O) gas or a nitrogen (N) gas can be used. 2 ) gas. By using an O-containing gas as the crystal growth inhibiting gas, at least a portion of the polycrystalline film formed on the surface of the wafer 200 in step A can be oxidized, and a film having a different film quality from the polycrystalline film and containing an element other than the element constituting the polycrystalline film, that is, an O layer, is formed on the surface of the polycrystalline film, thereby inhibiting continuous crystal growth. That is, the oxide layer can be used as the crystal growth inhibiting layer 500 that inhibits the crystal growth of the polycrystalline film.
[0111] In addition, when an oxygen-containing gas is used as a crystal growth inhibiting gas in step B, the oxygen (O) concentration of the film formed on the polycrystalline film after annealing described later is set to less than 1×10 23 [atoms / cm 3 Preferably, the peak value of the O concentration in the multilayer film before the annealing step is 1×10 20 ~1×10 22 [atoms / cm 3]. Alternatively, the process is carried out under conditions such that the crystal nuclei formed due to step B become a desired density, for example, the crystal grain size of the polycrystalline film formed on the polycrystalline film becomes a density that is 1 / 5 or more of the crystal grain size when step B is not performed. This can be achieved by controlling the oxygen partial pressure, the treatment temperature, the treatment time, etc. when supplying the O-containing gas in step B. As a result, the O concentration in the multilayer film becomes only a small amount compared to the stoichiometric composition, and the reduction of the crystal size is suppressed, and the influence on the characteristics of the multilayer film is limited.
[0112] [Step C]
[0113] By performing a cycle of performing the above-mentioned steps A and B non-simultaneously for a predetermined number of times (n times, where n is an integer greater than 1), a multilayer film having a predetermined thickness, for example, a thickness of 1 μm or more, is formed on the surface of the sacrificial layer 300 of the wafer 200. It is preferred that the above-mentioned cycle be repeated for a plurality of times. Specifically, a crystal growth inhibitory layer 500 is formed every time the polycrystalline film 400 is formed, for example, by 250 nm, thereby forming a multilayer film having a predetermined thickness, for example, a thickness of 1 μm or more, on the surface of the sacrificial layer 300 of the wafer 200. In addition, steps A and B may also be performed simultaneously.
[0114] Then, after step C, the above-mentioned step A is performed to form a polycrystalline film 400 on the crystal growth inhibiting layer 500. That is, the polycrystalline film 400 forms new crystal grains and accumulates on the crystal growth inhibiting layer 500. In other words, the polycrystalline film 400 on the upper and lower sides of the crystal growth inhibiting layer does not have crystal continuity or has its crystal continuity restricted.
[0115] In this way, Figure 4 As shown in (B) of FIG. 2 , the crystal grains of the polycrystalline film 400 on the wafer 200 are divided by the crystal growth inhibition layer 500 to form a multilayer polycrystalline film 400, i.e., a multilayer film. The structure of the multilayer film formed in this way is also referred to as ILIS (inhibition layer inserted structure), and the film forming process of forming such a structure is referred to as ILIS process. Figure 4 The single film structure of the prior art without using ILIS shown in (A) is called a comparative example. On the basis of obtaining a multilayer film of a specified film thickness, the above-mentioned specified number of times (the number of times step B is performed, also referred to as the number of crystal growth inhibitory layers) changes the density of the amorphous state or residual Si atoms described later in the entire multilayer film. Therefore, by controlling the specified number of times, the residual stress of the entire multilayer film can be controlled.
[0116] The above-mentioned prescribed number of times is set so that the absolute value of the residual stress in the multilayer film after the annealing process described later is within the range of an allowable value. The allowable value of the residual stress in the film varies depending on each application, but is, for example, -150 to 150 MPa. Here, the stress is set to be positive for tension and negative for compression. That is, by controlling the number of insertion steps B, the residual stress in the multilayer film after the annealing process can be controlled. Here, residual stress refers to the stress existing in an object in the absence of external force, and in the present disclosure, it can include the force acting between the multilayer film and its substrate, i.e., the wafer 200, and the stress remaining in the multilayer film after the sacrificial layer is removed and a portion of the residual stress is released. In addition, residual stress can also be referred to as film stress.
[0117] Here, the number of times step B is performed in the film forming process is set so that the greater the residual stress in the film after annealing, the greater the residual stress is, and the smaller the residual stress in the film is (i.e., greater on the compression side). In other words, by controlling the number of times step B is performed, the residual stress in the multilayer film can be controlled, and the residual stress of the multilayer film as a whole can be alleviated.
[0118] In addition, in the film forming process, by controlling the number of times step B is performed, the residual stress in the multilayer film can be controlled. Therefore, compared with the case where the number of times is fixed, the stress control range is wider, and even when the temperature in the annealing process described later is low (the thermal history is small), the residual stress can be set to a value close to 0.
[0119] (Purge and restore atmospheric pressure afterwards)
[0120] Next, inert gas is supplied from nozzles 249a to 249c into the processing chamber 201, respectively, and exhausted through exhaust port 231a. The inert gas supplied from nozzles 249a to 249c acts as a purge gas, thereby purging the processing chamber 201, and removing the remaining gas and reaction by-products from the processing chamber 201 (post-purge). After that, the gas atmosphere in the processing chamber 201 is replaced with an inert gas (inert gas replacement), and the pressure in the processing chamber 201 is restored to normal pressure (restoration of atmospheric pressure).
[0121] (Boat unloading and wafer unloading)
[0122] After that, the sealing cap 219 is lowered by the wafer boat lifter 115, and the lower end of the manifold 209 is opened. Then, the processed wafer 200 is carried out from the lower end of the manifold 209 to the outside of the reaction tube 203 while being supported by the wafer boat 217 (wafer boat unloading). After the wafer boat is unloaded, the gate 219s is moved, and the lower end opening of the manifold 209 is sealed by the gate 219s via the O-ring 220c (gate closing). After the processed wafer 200 is carried out to the outside of the reaction tube 203, it is taken out from the wafer boat 217 (wafer unloading).
[0123] Afterwards, in another processing furnace (processing chamber), the wafer boat is loaded, the pressure and temperature in the processing chamber are adjusted, and the next annealing step S120 is performed. That is, after the film forming step S110 is completed, the annealing step is performed in another processing furnace different from the processing furnace of the film forming step (ex-situ).
[0124] [Annealing step S120]
[0125] Next, the annealing step S120 will be described.
[0126] Here, for the wafer 200 on which a multilayer film is formed, the wafer 200 is subjected to a non-plasma N 2 Annealing treatment is performed in a gas atmosphere. Annealing treatment converts the initial film, i.e., the polycrystalline film, into films with different film qualities. Specifically, annealing treatment often expands the crystal grain size because it causes grain boundary movement or grain boundary sliding in the polycrystalline film. In addition, amorphous Si present near the grain boundary or in a certain crystal growth inhibitory layer is sometimes integrated with adjacent crystal grains based on the principle of solid phase epitaxial growth. As described later, through multiple experiments, it can be considered that the more times step B is performed, the higher the proportion of residual Si in the multilayer film as a whole, and the shrinkage rate caused by annealing treatment becomes larger. In addition, compared with the case where the crystal growth inhibitory layer 500 is not formed, the residual stress is transferred toward the 0 direction.
[0127] In addition, in step S120, the output of the heater is adjusted so that the temperature of the wafer 200 is higher than the temperature of the wafer 200 in the film forming step S110 and lower than 1200° C., more preferably higher than 900° C. and lower than 1100° C. The temperature of step S120 is set to be lower than the highest exposure temperature (typically 1100 to 1200° C.) during annealing when manufacturing the wafer 200 (i.e., before the film forming step S110), thereby suppressing changes in the characteristics of the wafer 200 such as the doping site or the concentration distribution of impurities. By setting it to lower than 1000° C., undesirable changes in the characteristics can be sufficiently suppressed.
[0128] In step S120, the more the prescribed number of step C in the above-mentioned film forming process S110 (the number of times step B is performed), the more the residual stress shifts from a negative value of compression to a positive value of tension. If it is assumed that the residual stress after annealing is a negative value when the prescribed number is 0, the more the prescribed number increases from 0 until the residual stress is reversed to positive, the smaller the absolute value of the residual stress in the multilayer film becomes. In other words, the annealing process S120 sets the temperature of the wafer 200 formed with the multilayer film to a temperature that changes the properties of the multilayer film in a manner that makes the number of step B in the above-mentioned film forming process S110 and the residual stress of the multilayer film after annealing have a positive correlation. Not only the maximum temperature, but also the heating rate and the cooling rate may affect the residual stress after annealing. If the film thickness of the multilayer film becomes thicker, for example, exceeding 10μm, it may be difficult to anneal uniformly in the depth direction by a method such as RTA (Rapid Thermal Anneal).
[0129] That is, in the annealing step S120, the absolute value of the residual stress of the multilayer film formed in the film forming step S110 performed by appropriately selecting the number of steps B can be made smaller than that before annealing, and the stress gradient is also reduced to improve the film quality. In this way, in the annealing step S120, the film can be changed into a film with improved film quality compared to the multilayer film before the annealing step, that is, the film can be changed into a film with improved film quality. In addition, in this context, the film quality may include part or all of the crystallographic, chemical, mechanical, optical, electrical and other various properties required in the formation of the device.
[0130] [Patterning Step S130]
[0131] Next, the patterning step S130 will be described.
[0132] Here, step S130 is performed in a processing furnace different from that in the film forming step S110 and the annealing step S120. In step S130, patterning is performed on the wafer 200 after the annealing process.
[0133] The patterning process includes resist coating, exposure, anisotropic etching, resist removal, and the like.
[0134] [Sacrificial Layer Removal Step S140]
[0135] Next, the sacrificial layer removing step S140 of removing the sacrificial layer will be described.
[0136] Here, a process of removing the sacrificial layer from the patterned wafer 200 using equipment different from that in the film forming process S110 , the annealing process S120 , and the patterning process S130 will be described.
[0137] As the sacrificial layer, for example, silicon oxide (SiO 2 ) layer, in SiO 2 The layer contains phosphorus (P) PSG layer, borophosphorus glass (BPSG: Boron phosphorus silicate glass, borophosphorus silicate glass) layer, Si layer, etc. 2 The layer can be obtained by a CVD method using tetraethoxysilane (TEOS) as a raw material or by thermal oxidation of the wafer 200. One or more of these can be used as the sacrificial layer.
[0138] In this step, the sacrificial layer formed as the base of the multilayer film on the wafer 200 is removed by chemical reaction with the etching gas. As the etching gas, for example, a halogen-containing gas can be used. As the halogen-containing gas, a fluorine (F)-containing gas can be used. As the etching gas, for example, by using a halogen-containing gas, the sacrificial layer formed on the wafer 200 can be removed. As an example of a halogen-containing gas, i.e., a F-containing gas, for example, hydrogen fluoride (HF) gas, chlorine trifluoride (ClF) gas, etc. can be used. 3 ) gas, chlorine fluoride (ClF) gas, nitrogen trifluoride (NF 3 ) gas, fluorine (F 2 ) gas, etc. As the F-containing gas, one or more of these can be used. In addition, the sacrificial layer can also be removed by wet treatment using a fluoric acid (HF) solution added with nitric acid, acetic acid, etc. In this case, as a solvent, a non-aqueous solvent such as hydrofluoroether can also be used in addition to water.
[0139] Here, when the sacrificial layer is removed and a structure such as a cantilever is formed, a polycrystalline film such as a polysilicon film formed on the sacrificial layer may sometimes warp in a direction perpendicular to the film. According to the present disclosure, since the polycrystalline film can be processed into a cantilever while maintaining the stress gradient of the polycrystalline film in the depth direction within a predetermined range and while reducing the absolute value of the residual stress in the film, the warping of the film can be suppressed.
[0140] In addition, this step is not limited to wet etching, and can also be performed by dry etching.
[0141] (3) Effects of this method
[0142] According to this aspect, one or more of the following effects can be obtained.
[0143] (a) By controlling the number of times the polycrystalline film on the wafer 200 is exposed to a crystal growth inhibiting gas, the residual stress in the multilayer film can be controlled and the film quality can be improved.
[0144] (b) The polycrystalline film on the wafer 200 is exposed to a crystal growth inhibiting gas, thereby controlling the grain size of the polycrystalline film. Specifically, regardless of the increase in the film thickness of the multilayer film, the uniformity of the grain size can be improved. In addition, a film with a small surface roughness can be obtained.
[0145] (c) In addition, in the subsequent annealing step, the residual stress in the multilayer film can be controlled within a desired range. Specifically, the absolute value or stress gradient of the residual stress in the multilayer film after annealing can be reduced.
[0146] (d) In the subsequent annealing step, the stress gradient in the multilayer film can be controlled within a desired range, thereby improving the film quality compared to before the annealing step. Specifically, the stress gradient in the multilayer film after annealing can be set to a value lower than an allowable value.
[0147] (e) In addition, since annealing is not performed during the film forming process and the processing temperature is not changed during the film forming process, the processing time can be shortened and the productivity can be improved.
[0148] (f) In addition, even when the sacrificial layer forming the base of the multilayer film on the wafer 200 is removed, the absolute value or gradient of the residual stress in the multilayer film can be reduced, so the warping of the multilayer film can be suppressed. Therefore, it can be suitably used in the manufacture of devices such as MEMS (Micro Electro Mechanical Systems).
[0149] (g) In addition, it is possible to use films formed by deposition to produce structures such as MEMS inertial sensors. Any film such as an electrode layer can be inserted under the multilayer film via a sacrificial layer, which can increase the degree of freedom in device design compared to SOI processes using silicon-on-insulator (SOI) wafers or cavity SOI wafers.
[0150] (h) In addition, a film having a thickness of 20 to 30 μm and a small absolute value or gradient of residual stress can be formed by the LPCVD method, which is excellent in mass productivity.
[0151] (4) Modification
[0152] Step B in this embodiment can be modified as shown in the following modifications. Unless otherwise specified, the processing procedures and processing conditions in each step of each modification can be the same as the processing procedures and processing conditions in each step of the above-mentioned substrate processing sequence.
[0153] In this modification, a predetermined gas that forms a film or surface having a different film quality from the polycrystalline film in step A is used instead of the crystal growth inhibiting gas in step B. That is, in the above-mentioned substrate processing apparatus, a predetermined gas supply system is provided for exposing the wafer 200 in the processing chamber 201 to the predetermined gas that forms a film having a different film quality from the polycrystalline film, and the processing sequence shown below is performed.
[0154] (raw material gas → specified gas) × n
[0155] The predetermined gas is, for example, a gas containing an element of Group 14. That is, the constituent elements of the polycrystalline film formed in step A and the constituent elements of the film having a different film quality from the polycrystalline film formed in step B may be substantially the same. For example, the film formed in step B may be a film having substantially the same composition as the initial film formed in step A except that the crystallinity is different.
[0156] Specifically, for example, in step B, the above-mentioned SiH 4 The silicon raw material gas other than the gas, for example, disilane (Si 2 H 6 ) gas or chlorosilane gas, and form an amorphous Si film having a different film quality from the polycrystalline film on the surface of the polycrystalline film formed on the wafer 200 in step A. By using a raw material gas different from the raw material gas in step A, the crystallinity can be made different without changing the temperature.
[0157] Even in this variation, the same effect as in the above-described method can be obtained. In addition, in this variation, in step B, a gas containing the same element as the element contained in the raw material gas in step A is used, so that the multilayer film does not contain elements different from the elements contained in the raw material gas.
[0158] Alternatively, the processes may be performed in parallel instead of being differentiated as in step A and step B. At this time, during the deposition, a predetermined gas different from the raw material gas is supplied together with the raw material gas in such a manner that the size of the crystal grains (cross-sectional area on a plane parallel to the substrate) does not change and / or the orientation is made the same, that is, in such a manner that the crystallinity is constant. At this time, the partial pressure of the raw material gas or the partial pressure of the predetermined gas exposed together with the raw material gas or the temperature of the wafer 200 is changed. Even in such a case, the gradient of the residual stress of the polycrystalline film can be maintained within a predetermined range, and the polycrystalline film can be processed into a cantilever while maintaining the stress gradient of the polycrystalline film within a predetermined range. Here, as the predetermined gas exposed together with the raw material gas, for example, N 2 Inert gas such as Ar or H 2 Gas, etc.
[0159] <Other aspects of the present disclosure>
[0160] The above specifically describes the embodiment of the present disclosure. However, the present disclosure is not limited to the above embodiment, and various modifications can be made without departing from the gist of the present disclosure.
[0161] For example, in the above-mentioned substrate processing step, although the structure of performing steps S110 to S140 in different processing furnaces (processing chambers) is described, it is not limited to this, and all steps or part of the steps can also be continuously performed in the same processing furnace (processing chamber) (i.e., in-situ processing). Even in this method, the same effect as the above method can be obtained.
[0162] In addition, for example, as the raw material gas used in step A, phosphine (PH) may be added (doped) to the Si-containing gas. 3 ), and form a doped Si film as a polycrystalline film. This makes it possible to adjust the flow rate of the doping gas for each nozzle and improve the surface uniformity of the impurity concentration. In addition, it is also possible to form a doped Si film each time and not add PH to the Si-containing gas. 3 When the undoped Si film is formed, a crystal growth inhibitory layer is formed and a multilayer film is formed. Even in this method, the same effect as the above method can be obtained.
[0163] In addition, for example, a nitrogen (N)-containing gas (also called a nitriding gas) may be used as the crystal growth inhibiting gas used in step B. As the N-containing gas, for example, nitric oxide (NO) gas or ammonia (NH 3 ) gas, N radicals, etc. In addition, the N-containing gas can also be activated by plasma, etc. As a result, at least a portion of the polycrystalline film formed on the surface of the wafer 200 in step A is nitrided, and a layer containing elements other than the elements constituting the polycrystalline film, namely N, is formed on the surface of the polycrystalline film, so that the crystal grains of the polycrystalline film can be terminated. That is, the nitride layer can also be used as a crystal growth inhibitory layer of the polycrystalline film. Even in this method, the same effect as the above method can be obtained.
[0164] In addition, for example, the film formed in step A is not limited to a polycrystalline film, but may also be an amorphous film or a single crystal film. In addition, the film formed in step B can be arbitrarily selected from polycrystalline films, amorphous films, etc. whose crystallinity is different from that of step A. In the case where the initial film is an amorphous film, the laminated film is easily polycrystallized by annealing at 600°C or above. At this time, the treatment of step B can help with nucleation, grain boundary formation, and grain size control. In addition, the film formed in step B only needs to be different from the surface state in the process of step A in at least one atomic layer on the surface, and further, it does not need to be a continuous film. That is, step B is not limited to depositing a new film on the initial film deposited by step A, and the surface of the initial film can also be reconstructed, or a very small part of the surface (scatteredly) adsorbs a specified molecule, or is modified by chemical reaction, or the atomic bond is cut, or excited. Even in this method, the same effect as the above method can be obtained.
[0165] In addition, in the above-mentioned substrate processing step, although the case of forming a multilayer film on the wafer 200 with a sacrificial layer formed thereon is described as an example, the present disclosure is not limited thereto, and can also be appropriately applied to the case where the sacrificial layer is not in direct contact with the wafer 200, and the case where the multilayer film is not in direct contact with the sacrificial layer. The sacrificial layer is not limited to a silicon oxide film, but may also be a nitride film wafer, and may also be any of an amorphous film and a crystalline film. SiO 2 The film is usually amorphous, but may include microcrystals having an orientation corresponding to the crystal orientation of the substrate. In this case, the multilayer film formed on the microcrystals may also have an orientation corresponding to the crystal orientation of the substrate.
[0166] In addition, in the above-mentioned substrate processing step, although the case where a polycrystalline film is formed by a uni-element semiconductor composed only of Si is used as an example, the present disclosure is not limited to this, and can also be applied to mixed crystals or compound semiconductors such as SiGe. In addition, the annealing treatment is not limited to heating the multilayer film as a whole to a specified temperature, and the surface side can also be set to a higher temperature and greatly reduced by RTA and other techniques to form a stress gradient such as warping the cantilever upward. In addition, the formation of the polycrystalline film is not limited to thermal CVD, and plasma CVD, optical CVD, reactive CVD or other various film forming methods that can form a polycrystalline film can also be used.
[0167] In addition, the recipes used in each process are preferably prepared individually according to the process content, and are pre-stored in the storage device 121c via the electrical communication line or the external storage device 123. And, when starting each process, it is preferred that the CPU 121a selects a suitable recipe from the plurality of recipes stored in the storage device 121c according to the process content. This makes it possible to form films of various film types, composition ratios, film qualities, and film thicknesses with good reproducibility by using one substrate processing device. In addition, it is possible to reduce the burden on the operator and start each process quickly while avoiding operational errors.
[0168] In addition, the above-mentioned recipe is not limited to the case of re-generation, and can also be prepared by, for example, changing an existing recipe installed in the substrate processing device. In the case of changing the recipe, the changed recipe can be installed in the substrate processing device via an electrical communication line or a recording medium recording the recipe. In addition, the input / output device 122 of the existing substrate processing device can be operated to directly change the existing recipe installed in the substrate processing device.
[0169] In addition, in the above-mentioned manner, an example of forming a film using a batch-type substrate processing device that processes multiple substrates at a time is described. The present disclosure is not limited to the above-mentioned manner, and can also be appropriately applied to the case where a film is formed using a single-piece substrate processing device that processes one or more substrates at a time. In addition, in the above-mentioned manner, an example of forming a film using a substrate processing device having a hot wall type processing furnace is described. The present disclosure is not limited to the above-mentioned manner, and can also be appropriately applied even when a film is formed using a substrate processing device having a cold wall type processing furnace.
[0170] Even when these substrate processing apparatuses are used, each process can be performed by the same process procedure and process conditions as those in the above-mentioned embodiment, and the same effects as those in the above-mentioned embodiment can be obtained.
[0171] In addition, the above-mentioned various modes and modified examples can be used in combination as appropriate. The processing process and processing conditions at this time can be set to be the same as the processing process and processing conditions of the above-mentioned modes and modified examples, for example.
[0172] (5) A number of experimental results are described below.
[0173] (Experiment 1)
[0174] The above-mentioned film forming step (ILIS process) and annealing step were performed using the above-mentioned substrate processing apparatus, and an evaluation sample in which a multilayer film was formed on a sacrificial layer of a wafer was produced. Figure 6The graph shows the results of analyzing the O concentration in the film of the evaluation sample by secondary ion mass spectrometry (SIMS). The processing conditions in each step when preparing the evaluation sample were set to predetermined processing conditions within the range of the processing conditions in each step of the above-mentioned method. Figure 6 The horizontal axis of the graph represents the depth of the film, the right vertical axis represents the secondary ion intensity of Si, and the left vertical axis represents the O concentration. In addition, in the above-mentioned step B, when the O of the crystal growth inhibiting gas is supplied, 2 The O concentration in the multilayer film after annealing is less than 1×10 23 [atoms / cm 3 ] under the treatment conditions.
[0175] Oxygen (O) is the most abundant element in the film composition after Si. It was confirmed that the peak (maximum) of the O concentration in the multilayer film after annealing was at 1×10 20 ~1×10 22 [atoms / cm 3 ] between. In addition, it is confirmed that the supply O 2 The O concentration in the multilayer film when the gas is used is compared with that in the SiO 2 The O concentration slope at the interface of the layer is relatively gentle. This is believed to be because the surface roughness (maximum height roughness) of the multilayer film is about 50 to 100 nm and O has diffused during film formation. In addition, it was confirmed that the typical O concentration in the polycrystalline film after annealing is less than 1×10 17 [atoms / cm 3 This is lower than the typical residual oxygen concentration of 1×10 18 [atoms / cm 3 ] and is less than the solid solubility limit of O. In addition, the sample without annealing process was also measured, and the result showed that there was no significant difference in the profile curve of O concentration.
[0176] Therefore, it was confirmed that the O concentration in the multilayer film formed by the present substrate processing step was extremely low and did not cause any hindrance while being able to satisfy the film quality required for the multilayer film for MEMS. 23 [atoms / cm 3 ] or more, the grain size and resistivity will decrease, and the required film quality may not be met after annealing. However, if the 22 [atoms / cm 3 ], the effect on the film quality is limited. In addition, if the O concentration is less than 1×10 20[atoms / cm 3 ], the crystal growth inhibition effect is not sufficient, new crystal grains cannot be formed, and stress control may become difficult. However, if it is 1×10 20 [atoms / cm 3 ] or above, a sufficient crystal growth inhibitory effect for stress control can be obtained.
[0177] (Experiment 2)
[0178] Figure 7 This is a graph showing the relationship between the number of times a crystal growth inhibiting gas is supplied and the residual stress in the film when the above-mentioned ILIS process is performed using the above-mentioned substrate processing apparatus and a multilayer film with a film thickness of 1 μm is formed on the wafer, and comparing the case where no annealing step is subsequently performed and the case where an annealing step is subsequently performed. Figure 7 The horizontal axis represents the number of times the crystal growth hindering gas is supplied for every 1 μm of film thickness, and the vertical axis represents the residual stress in the multilayer film. In the figure mark of the residual stress, negative represents compressive stress and positive represents tensile stress. The internal stress of the multilayer film is evaluated by the substrate curvature method, which is to peel off the single-sided multilayer film after the film forming process is performed on both sides of the substrate and measure the warping of the substrate. In addition, the number of supplies of 1, 3 and 9 times respectively indicates that there is a crystal growth hindering layer when the depth of the multilayer film from the surface increases by 500nm, 250nm and 100nm.
[0179] In the absence of the annealing step, the residual stress in the multilayer film is all negative (compressive stress). Furthermore, it was confirmed that the compressive stress increases as the number of times the crystal growth inhibiting gas is supplied increases.
[0180] In contrast, in the presence of an annealing process, in all supply times, compared to the case where there is no annealing process, the residual stress in the multilayer film changes toward the stretching side, and the absolute value becomes smaller. It is further confirmed that the more times the crystal growth hindering gas is supplied, the residual stress (compressive stress) will move significantly toward the stretching direction, and the residual stress is closer to 0. That is, it is confirmed that the absolute value of the residual stress in the multilayer film on the wafer can be reduced according to the supply times of the crystal growth hindering gas. That is, in the absence of an annealing process and in the case of an annealing process, the dependence of the residual stress on the number of hindering layers will be reversed. It can be considered that the mechanism will be as follows. First, as an important factor for easing the residual stress by annealing, it can be considered to be the shrinkage of the film. Specifically, a model such as the residual Si atoms present in the grain boundary are introduced into the crystallization. The remaining Si is an amorphous Si present between the crystal and the crystal, and since it is not crystallized, the density is small. When the annealing process is performed, the originally amorphous part will crystallize, and the volume will decrease, and the residual stress will change from the compression side to the tension side. When a large compressive stress remains in a film immediately after deposition, the absolute value of the residual stress becomes smaller than that before annealing due to annealing.
[0181] Next, it can be considered that the important factor that causes the difference in the tendency to depend on the number of barrier layers before and after annealing is the difference in the number of grain boundaries. Here, it is assumed that the more the polycrystalline film 400 is deposited, the larger the size of the crystal grains becomes. Therefore, by increasing the number of barrier layers, the unit thickness of each layer of the polycrystalline film becomes smaller, and the average grain size becomes smaller. This will lead to an increase in the area of the grain boundaries and an increase in the proportion of remaining atoms, and the residual stress of the just deposited film will increase toward the compression side. On the other hand, when annealing is performed, the more barrier layers there are, the higher the shrinkage rate becomes, and the residual stress will be greatly relaxed and change to the tensile side. This model can be further verified by experiments 3 to 4 described later.
[0182] That is, it was confirmed that by performing the annealing treatment, the residual stress will be relaxed compared to the case where the annealing treatment is not performed, and further, the more times the crystal growth inhibiting gas is supplied, the residual stress in the film will be transferred to the tensile direction due to the compressive stress, and the residual stress can be made closer to 0. In other words, it was confirmed that after the annealing treatment, the properties of the multilayer film will be changed, so that the more times the crystal growth inhibiting gas is supplied, the greater the residual stress in the film becomes, or the absolute value of the residual stress becomes smaller. In this way, once a multilayer film with a large compressive stress, that is, a film quality that is not preferred, is formed by the crystal growth inhibiting layer, and the cause of the compressive stress is removed by annealing, a film with excellent film quality compared to a film without a crystal growth inhibiting layer can be obtained.
[0183] In addition, in other experiments in which the film forming process was performed at 620°C and the annealing process was performed at 900°C for 1 hour, it was confirmed that the residual stress after annealing was substantially zero or only a small amount of positive residual stress. Therefore, it can be considered that by further optimizing the film forming process temperature and the annealing process temperature and time, the residual stress can be made closer to zero, or the tensile stress can be made to remain. Figure 7 In the invention, it is suggested that the control range of residual stress can be expanded to about 2 times by including an option of not performing annealing (i.e., making the annealing temperature as close to the film forming temperature as possible). For example, when the target stress is less than the specified stress, stress control can be performed in a manner that the stress decreases as the number of sacrificial layers increases without performing annealing, and when the target stress exceeds the specified stress, stress control can be performed in a manner that the stress increases as the number of sacrificial layers increases. Thus, when it is desired to give a specified warp to the cantilever, the control range of the warp can be expanded.
[0184] (Experiment 3)
[0185] In Experiment 3, a 100 μm thick base SiO 2 " was used as a sacrificial layer on both sides of a 200 mm Si wafer, and a 1 μm multilayer film was formed under two conditions using the above-mentioned substrate processing device, and evaluated by cross-sectional TEM (Transmission Electron Microssopy) observation and XRD (X-Ray Diffraction). Here, sample 1 and sample 2 were prepared by the first of the two conditions. That is, Figure 8 As shown in (A) of the comparative example, in the film forming process, a PH 3 The process of forming a doped Si film 600a with a thickness of 25 nm by using Si-containing gas, and the process of not adding PH 3 The process of forming a non-doped Si film 600b with a thickness of 225 nm was performed four times to form a polycrystalline film 600. Samples 3 and 4 were produced under the second condition. Figure 8 As shown in (B) in FIG. 1 , by using a sacrificial layer 300 with PH added thereto each time 3 The process of forming a doped Si film 600a with a thickness of 25 nm by using Si-containing gas, and the process of not adding PH 3 In the process of forming the undoped Si film 600b with a thickness of 225 nm, O 2 gas and forms a crystal growth barrier (also called O 2The polycrystalline film 600 is formed by an ILIS process with a purge layer of 500”. Both conditions are that the film forming temperature of the polycrystalline film is 620°C, and the phosphorus concentration in the phosphorus-doped Si film 600a is 1×10 20 [cm -3 ], for samples 2 and 4, in N 2 Annealing treatment was performed at 1100° C. for 5 minutes in a gas atmosphere.
[0186] Fig. 9 (A) shows a cross-sectional TEM image of sample 1. Fig. 9 (B) shows a cross-sectional TEM image of sample 3. Sample 1 has changed its pattern in the depth direction, with irregular crystals near the base oxide film, and it is confirmed that it grows into columnar crystals with the subsequent increase in film thickness. In contrast, it can be confirmed that the crystal growth of sample 3 is hindered by the crystal growth hindering layer, making the crystallinity in the film thickness direction uniform.
[0187] Fig.10 (A) shows a cross-sectional TEM image of sample 2. Fig.10 (B) in the figure shows a cross-sectional TEM image of sample 4. It can be confirmed that sample 2 has a large growth in grain size by annealing. On the other hand, in sample 4, even if annealing is performed, crystal growth will be suppressed due to the barrier layer. In either case, single crystalization is not caused by annealing. When the remaining Si atoms are introduced into the crystal by reducing the grain boundaries, it can also be expected that the compressive stress caused by the remaining Si atoms will be reduced. In this case, the higher the annealing temperature, the greater the reduction in compressive stress.
[0188] Fig.11 (A) is a diagram showing the XRD spectrum of sample 2. Fig.11 (B) in the figure is a diagram showing the XRD spectrum of sample 4. Both were measured by the in-plane method. Compared with the spectrum obtained from the powder, the intensity of (111) of sample 2 is stronger, so that it can be confirmed that there is a clear crystal orientation. On the other hand, although sample 4 has orientation, the proportion of (111) is smaller than that of sample 1. It can be considered that this is because the growth of (111) crystals that grow with the increase in film thickness is hindered.
[0189] (Experiment 4)
[0190] In Experiment 4, a 2 μm thick SiO substrate was formed on both sides. 2 The two sides of the 200 mm Si wafer were used as sacrificial layers, and a 25 μm multilayer film was formed using the above substrate processing device under the above two conditions. Samples 1 and 2 were produced under the first condition. That is, Figure 8As shown in (A) of the comparative example, in the film forming process, a PH 3 The process of forming a doped Si film 600a with a thickness of 25 nm by using Si-containing gas, and the process of not adding PH 3 The process of forming the undoped Si film 600b with a thickness of 225 nm was performed 100 times to form the polycrystalline film 600. Samples 3 and 4 were produced under the second condition. Figure 8 As shown in (B) in FIG. 1 , by using a sacrificial layer 300 with PH added thereto each time 3 The process of forming a doped Si film 600a with a thickness of 25 nm by using Si-containing gas, and the process of not adding PH 3 In the process of forming the undoped Si film 600b with a thickness of 225 nm, O 2 The polycrystalline film 600 is formed by an ILIS process in which the gas is removed and the crystal growth inhibitory layer 500 is formed.
[0191] And, for samples 1 and 3, in N 2 The samples 2 and 4 were annealed at 900°C for 60 minutes in a N 2 Annealing treatment was performed at 1100°C for 5 minutes in a gas atmosphere. In addition, photolithography, deep reactive ion etching, and sacrificial layer removal were performed on samples 1 to 4, respectively, to form various cantilevers with a width of 18 μm and a length of 100 to 700 μm, and the cantilevers were evaluated.
[0192] Fig.12 (A) is the cross-sectional SEM image of sample 2. Fig.12 (B) is a cross-sectional SEM image of sample 4. In order to confirm the crystallinity dependent on depth in this cross section, the underlying SiO 2 EBSD analysis was performed on the 5 μm section of the interface. Fig.13 (A) Fig.13 As shown in (B) in FIG. 1 , the observation field of the EBSD analysis is set to be divided into three regions of upper, middle, and lower regions 5 μm from the interface.
[0193] Fig.14 The anti-pole diagram orientation mapping of sample 2 and sample 4. The anti-pole diagram represents the orientation of the crystal at each position in the field of view as a shade corresponding to the surface index of a certain crystal plane that is perpendicular to the cross section of the sample. The grain size at each field of view calculated based on the mapping is shown in Table 1. In addition, the grain size is calculated as a weighted average grain size (μm) based on the area ratio. In this calculation, the boundary of the twin crystal is not regarded as a grain boundary.
[0194] [Table 1]
[0195] Field of view Sample 2 Sample 4 superior 0.46 0.16 central 0.38 0.17 Down 0.32 0.17
[0196] According to Table 1, the grain size of sample 2 increases with film growth, but the grain size of sample 4 does not depend on the depth direction. In addition, it can be seen that the crystal shape of sample 2 is different in the depth direction, while the crystal growth of sample 4 is suppressed and uniform in the depth direction.
[0197] Fig.15 This is the anti-pole diagram mapping of sample 2 and sample 4. This mapping shows the proportion of the crystal plane in each field of view in the unit triangle of the stereographic projection as light and dark. Fig.15 It can also be seen that the distribution of crystal orientation in the depth direction of sample 2 is uneven, but the distribution of crystal orientation in the depth direction of sample 4 is uniform. Based on these results, it can be seen that the crystal grain size, crystal shape, and crystal orientation in the depth direction of sample 4 produced by the ILIS process are more uniform than those of the comparative example sample 2. Therefore, the density of the remaining Si will also be uniform, and it can be expected that the stress gradient will be small.
[0198] Fig.16 (A) is a diagram showing a SEM image of a cantilever produced using sample 2. Fig.16 (B) is a diagram showing a SEM image of a cantilever produced using sample 4. In addition, two types of cantilevers, 700 μm in length and 500 μm in length, were evaluated as simple one-sided support beams. Fig.16 (A) and Fig.16 (B) in the figure has a length of 700 μm.
[0199] Fig.17 is a graph showing a contour curve of the displacement of the cantilever surface. As shown, the displacement is measured in the vertical direction of the wafer 200 using a white interferometer. Fig.16 The 700 μm cantilever of sample 2 shown in (A) has a large warp that touches the Si substrate, and the pressure gradient is calculated based on the 500 μm cantilever. Fig.16 The 700 μm cantilever of sample 4 shown in (B) shows a profile curve that is almost consistent with the 500 μm cantilever. The cantilever tip only moves 0.8 μm downward, and the calculated pressure gradient is confirmed to be only -0.65 MPa / μm, which is very small. It can be seen that ILIS will play a role in easing the pressure gradient. In addition, the stress gradient X is calculated according to the following formula.
[0200] [Number 1]
[0201]
[0202] In the above, u is the change in the longitudinal direction of the cantilever, L is the length of the cantilever, E is the Young's modulus, ν is the Poisson's ratio of polysilicon (a well-known value, i.e., 0.22), and the value obtained by measuring the polycrystalline film of the sample using a nanoindenter is used for the Young's modulus.
[0203] Table 2 shows the indicators of sample 2, sample 4 and a known Epi-poly Si film. The residual stress was calculated by measuring the displacement of the front end of the cantilever in the long side direction (i.e., the extension and contraction of the cantilever) using a rotating beam structure and multiplying it by the Young's modulus. The surface roughness was measured as the arithmetic mean roughness by atomic force microscopy (AFM). The resistivity was measured by spreading resistance profiling (SRP).
[0204] [Table 2]
[0205]
[0206] The absolute value of the stress gradient X of sample 4 is smaller than the absolute value of the stress gradient X of sample 2. In addition, the absolute value of the residual stress of sample 4 is smaller than the absolute value of the residual stress of sample 2. In addition, the surface roughness (also referred to as surface roughness) of sample 4 is smaller than the surface roughness of sample 2. That is, by hindering the crystal growth with a crystal growth barrier layer and forming uniform crystallinity in the depth direction, the absolute value of the residual stress and the stress gradient can be reduced, and the surface roughness will also be reduced. According to the above content, it is confirmed that by forming a crystal growth barrier layer, the warping of the polysilicon film of the cantilever structure can be reduced, so that the polysilicon film can be applied to MEMS. In addition, the resistivity of both samples 2 and 4 is worse than that of the known Epi-polySi film, and the deterioration of sample 4 is more serious. As the reason, in addition to the expansion of the crystal grain size, it can also be considered that there is a lack of optimization of the process conditions. Since the ILIS of this example is a technology based on the well-known LPCVD polycrystalline Si, the resistivity can be easily adjusted.
[0207] Description of Reference Numerals
[0208] 121 controller (control unit)
[0209] 200 wafers (substrates).
Claims
1. A substrate processing method, characterized in that: have: A step of forming a multilayer film having a predetermined thickness on a substrate by performing a cycle including (a) and (b) a predetermined number of times, The (a) is a step of depositing an initial film by exposing the substrate to a raw material gas; The step (b) is a step of exposing the substrate to a crystal growth inhibiting gas or a predetermined gas that forms a film having a different film quality from the initial film. The predetermined number of times is set so that after the multilayer film is annealed, an absolute value or a gradient of residual stress of the multilayer film is smaller than an allowable value.
2. The substrate processing method according to claim 1, characterized in that: (a), a polycrystalline film is deposited as the initial film, (b) is performed under the conditions that the polycrystalline film deposited in (a) forms new crystal grains.
3. The substrate processing method according to claim 1, characterized in that: The initial film contains a Group 14 element.
4. The substrate processing method according to claim 1, characterized in that: In (b), by exposing the substrate to the crystal growth inhibiting gas, crystal nuclei are provided at a predetermined density to the initial film to be deposited in the subsequent (a).
5. The substrate processing method according to claim 1, characterized in that: The crystal growth hindering gas is an oxygen-containing gas.
6. The substrate processing method according to claim 1, characterized in that: The predetermined gas contains a Group 14 element, and constituent elements of the initial film and constituent elements of a film having a different film quality from the initial film are substantially the same.
7. The substrate processing method according to claim 1, characterized in that: (a) and (b) were performed at the same temperature.
8. The substrate processing method according to claim 1, characterized in that: In (b), a layer containing elements other than the elements constituting the initial film is formed on the surface of the initial film formed in (a) immediately before.
9. The substrate processing method according to claim 5, characterized in that: (b) The oxygen concentration in the film having a different film quality from the initial film after annealing is less than 1×10 23 [atoms / cm 3 ] under the treatment conditions.
10. The substrate processing method according to claim 6, characterized in that: The initial film is a polycrystalline film, and the film having a different film quality from the initial film is an amorphous film.
11. The substrate processing method according to claim 1, characterized in that: The thickness of the film or layer formed in (b) is thinner than the thickness of the initial film formed in the immediately preceding step (a).
12. The substrate processing method according to claim 11, characterized in that: The thickness of the film or layer formed in (b) is 1 / 10 or less of the thickness of the initial film formed in (a) immediately before.
13. The substrate processing method according to claim 1, characterized in that: The predetermined number of times is set to be greater when the residual stress after annealing is greater, and to be less when the residual stress is smaller.
14. The substrate processing method according to claim 1, characterized in that: The substrate processing method further comprises (c), The step (c) is a step of annealing the multilayer film at a temperature below 1200° C., In (c), the multilayer film is changed so that the absolute value of the residual stress after annealing becomes smaller as the predetermined number of times increases from 0.
15. The substrate processing method according to claim 14, characterized in that: The crystal growth hindering gas is an oxygen-containing gas, The maximum oxygen concentration in the multilayer film after (c) is 1×10 20 ~1×10 22 [atoms / cm 3 ]between, The oxygen concentration in the initial film after (c) is less than 1×10 18 [atoms / cm 3 ].
16. The substrate processing method according to claim 14, characterized in that: The surface of the substrate before the initial (a) has a sacrificial layer, The substrate processing method further comprises (d), The step (d) is a step of removing the sacrificial layer after step (c).
17. A substrate processing method, characterized in that: With (a) and (b), The step (a) is a step of exposing a single crystal substrate having an oxide film formed on the surface thereof to a gas containing a first element in a processing chamber, and depositing a polycrystalline film containing the first element on the surface thereof in a manner such that at least a portion of crystal grains are epitaxially grown on the single crystal substrate; The step (b) is a step of processing the polycrystalline film into a cantilever while maintaining the stress gradient of the polycrystalline film within a predetermined range. (a) includes a step of changing the partial pressure of the gas containing the first element or the partial pressure of a gas different from the gas containing the first element exposed together with the gas containing the first element, or the temperature of the single crystal substrate in such a manner that the crystallinity is constant during the deposition.
18. A method for manufacturing a semiconductor device, characterized in that: have: A step of forming a multilayer film having a predetermined thickness on a substrate by performing a cycle including (a) and (b) a predetermined number of times, The (a) is a step of depositing an initial film by exposing the substrate to a raw material gas; The step (b) is a step of exposing the substrate to a crystal growth inhibiting gas or a predetermined gas that forms a film having a different film quality from the initial film. The predetermined number of times is set so that after the multilayer film is annealed, an absolute value or a gradient of residual stress of the multilayer film is smaller than an allowable value.
19. A substrate processing device, characterized in that: have: a processing chamber that processes the substrate; a raw material gas supply system, which exposes the substrate in the processing chamber to the raw material gas; a crystal growth inhibiting gas supply system or a specified gas supply system, wherein the crystal growth inhibiting gas supply system exposes the substrate in the processing chamber to a crystal growth inhibiting gas, and the specified gas supply system exposes the substrate in the processing chamber to a specified gas, wherein the specified gas is used to form a film having a different film quality from an initial film deposited by exposing the substrate in the processing chamber to the raw material gas; a control unit configured to control any one of the raw material gas supply system, the crystal growth inhibiting gas supply system, and the specified gas supply system so as to perform a process of forming a multilayer film of a specified thickness on the substrate by performing a cycle including (a) and (b) a specified number of times in the processing chamber, The (a) is a process of causing initial film deposition by exposing the substrate to the raw material gas; The (b) is a process of exposing the substrate to the crystal growth inhibiting gas or the predetermined gas. The predetermined number of times is set so that after the multilayer film is annealed, an absolute value or a gradient of residual stress of the multilayer film is smaller than an allowable value.
20. A program, which causes a substrate processing apparatus to execute, in a processing chamber of the substrate processing apparatus, a process of forming a multilayer film of a predetermined thickness on a substrate by performing a cycle including (a) and (b) a predetermined number of times, through a computer, The (a) is a process of depositing an initial film by exposing the substrate to a raw material gas; The (b) is a process of exposing the substrate to a crystal growth inhibiting gas or a predetermined gas that forms a film having a different film quality from the initial film. It is characterized in that The predetermined number of times is set so that after the multilayer film is annealed, an absolute value or a gradient of residual stress of the multilayer film is smaller than an allowable value.