Method for preparing copper-chromium consumable electrode
By adopting low-temperature sintering and crushing processes in the preparation of copper-chromium contact materials, the powder separation and agglomeration problems are solved, and the composition of copper-chromium self-consumable electrodes is uniform and dense, improving the performance of vacuum circuit breaker contacts and Finished rate.
Patent Information
- Application Number
- CN202411191279.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the copper-chromium contact material is uneven in the preparation process due to powder separation and agglomeration, and the sintering strength is poor, resulting in local copper-rich/chromium-rich defects, loosening and block loss in the contact material in the vacuum circuit breaker. , the yield rate is low.
The method of preparing copper-chromium self-consumable electrodes using vacuum metal covers includes weighing copper powder and chromium powder according to the process requirements and sintering in a reducing atmosphere at low temperature, crushing into sintered powder, and then filling into the metal cover. Perform vacuum sintering to ensure uniform composition and high density.
The copper chromium self-consumable electrode prepared by this method has high density and uniform composition. It is used for vacuum self-consumable arc smelting and stable smelting process. The metallographic structure of the product is uniform, without loose or block loss defects, and the yield rate can reach more than 92% .
Smart Images

Figure CN119035549A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy material preparation, and in particular to a method for preparing a copper-chromium consumable electrode. Background Art
[0002] Copper-chromium contacts (CuCr contacts, chromium content is usually 25-55% by mass) have the characteristics of high voltage resistance, large breaking current capacity, low cutoff value, good anti-welding performance, etc. They are widely used in vacuum circuit breakers and are currently the main contact material for vacuum circuit breakers. There are four main methods for preparing copper-chromium contacts: solid phase sintering, infiltration, casting and vacuum consumable arc melting (arc melting for short). Among them, the copper-chromium contacts manufactured by arc melting have the best comprehensive performance and are currently recognized as the copper-chromium contacts with the best performance in the world.
[0003] The preparation technology of consumable electrodes is the key to the production of copper-chromium contact materials by arc melting. The process of preparing consumable electrodes using metal sheaths is as follows: mixing chromium powder and copper powder - loading the mixed powder into the metal sheath - vacuum sintering. Due to the difference in particle size and particle morphology between copper powder and chromium powder, powder separation and agglomeration are likely to occur when loading the mixed powder, resulting in uneven composition of the consumable electrode, and ultimately leading to local copper-rich / chromium-rich defects in the contact material; in addition, due to the poor sintering strength at the chromium powder aggregation site of the consumable electrode, the original powder particles are likely to fall off into the molten pool during arc melting, and even powder blocks may fall directly into the molten pool, causing defects such as looseness and falling blocks in the contact material.
[0004] The invention patent with publication number CN1041975A discloses a method for manufacturing a molten material composed of copper, chromium and at least one easily evaporable component and a consumable electrode used in the method, wherein the electrode structure is composed of a copper tube, a copper-chromium powder mixture is placed in the copper tube, and a solid part composed of a copper-tellurium alloy, a copper-selenium alloy or a copper-antimony alloy is arranged in the copper-chromium powder mixture. The invention summarizes the basic structure of the copper tube consumable electrode, and the copper powder, chromium powder and copper alloy solid part used have differences in particle size and morphology, and are prone to component separation or agglomeration during filling, thereby making the composition of the consumable electrode uneven, and ultimately causing the defect of local enrichment of the contact material; at the same time, the consumable electrode with uneven composition has poor sintering strength, and the powder or solid part is easy to fall off and fall into the molten pool during the arc melting process, causing the contact material to have defects such as looseness and falling blocks, and the yield rate is low. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing a copper-chromium consumable electrode by using a vacuum metal sheath. The consumable electrode prepared by this method has high density and uniform composition.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A method for preparing a copper-chromium consumable electrode comprises the following steps:
[0008] 1) Weigh the corresponding amount of copper powder and chromium powder according to the alloy composition required by the process and set aside;
[0009] 2) The weighed copper powder and chromium powder are mixed evenly, the obtained mixed powder is sintered at low temperature in a reducing atmosphere, and the obtained sintered material is crushed to obtain a sintered powder; wherein the low temperature sintering is carried out at a temperature of 300 to 550° C.;
[0010] 3) The obtained sintered powder is filled into a metal sheath, and after compaction, it is placed under vacuum conditions for vacuum sintering to obtain the copper-chromium consumable electrode.
[0011] In the industry, the composition of copper-chromium contact materials is usually 75-45% copper and 25-55% chromium by weight. Therefore, in step 1) of the method of the present invention, copper powder and chromium powder are weighed at 75-45% and 25-55% by weight, respectively. In the present invention, the copper powder is usually electrolytic copper powder, which has a dendritic shape and a particle size of ≤75μm (usually 200-mesh or 300-mesh sieve); the chromium powder is usually obtained by mechanical crushing of chromium blocks, has an irregular shape, and a particle size of 75-150μm (about 100-200 mesh).
[0012] In step 2) of the above preparation method, the copper powder and the chromium powder are mixed uniformly by conventional methods, such as placing the weighed copper powder and chromium powder in a mixer and mixing for 2 to 5 hours or even longer to achieve uniform mixing of the two. After low-temperature sintering, the sintered material is usually crushed to less than or equal to 40 mesh, preferably crushed to 40 to 60 mesh. The reducing atmosphere is usually a hydrogen atmosphere.
[0013] The applicant has found that low-temperature sintering of the mixed powder can make the copper powder and chromium powder in the mixed powder have a certain bonding effect, and obtain a sintered material (sintered block) with a certain sintering strength between the copper powder and the chromium powder. Since the copper powder and the chromium powder in the mixed powder are mixed evenly, the components in the sintered material obtained after sintering the mixed powder are also uniform; the sintered material is subsequently crushed to break the irregular large-sized block-shaped sintered blocks into small-sized sintered powders with uniform sizes. On the one hand, the small-sized sintered powders have better sintering strength than the large-sized sintered blocks. On the other hand, even after crushing, since the sintered material itself has a certain sintering strength and is crushed to 40-60 mesh, the crushed particle size is much larger than the particle size of the copper powder and chromium powder raw materials themselves. Therefore, when the sintered powder obtained after crushing is filled into the metal sheath, it is not easy for the copper powder and chromium powder to separate, the copper powder to agglomerate or the chromium powder to agglomerate, thereby making the composition of the obtained consumable electrode uniform and the density high.
[0014] In step 3) of the above preparation method, the metal sheath may be a sheath made of metal material in a conventional shape such as a tube or a square, such as a copper tube, a chrome bronze tube, etc.
[0015] In step 3) of the above preparation method, the vacuum sintering is carried out in a conventional vacuum sintering furnace, and the sintering parameters are the same as those in the prior art, preferably: the vacuum reading is ≤0.01Pa, and the vacuum sintering is carried out at 900-1050°C. Under the above conditions, the holding time of vacuum sintering is usually ≥1h, and the holding time is further preferably 1.5-6h.
[0016] Compared with the prior art, the present invention adopts a process combination of "powder mixing-low temperature sintering-crushing", which solves the powder separation / aggregation problem that occurs in the process of directly filling the mixed powder into the metal sheath in the prior art, so that the consumable electrode obtained is dense and has uniform composition. When it is used for vacuum consumable arc melting, the stability of the melting process can be greatly improved, and the metallographic structure of the copper-chromium contact product obtained is uniform, without looseness, falling blocks and copper-rich / chromium-rich defects of more than 100μm, and the product yield can reach more than 92%. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 25 consumable electrode prepared in Example 1 of the present invention.
[0018] Figure 2 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 25 consumable electrode prepared in Comparative Example 1 of the present invention.
[0019] Figure 3This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 40 consumable electrode prepared in Example 2 of the present invention.
[0020] Figure 4 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 40 consumable electrode prepared in Comparative Example 2-1 of the present invention.
[0021] Figure 5 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 40 consumable electrode prepared in Comparative Example 2-2 of the present invention.
[0022] Figure 6 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 55 consumable electrode prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0023] In order to better explain the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments, but the embodiments of the present invention are not limited thereto.
[0024] Example 1
[0025] 1) Weigh 75% of copper powder and 25% of chromium powder by weight and set aside;
[0026] 2) The weighed copper powder and chromium powder are placed in a mixer and mixed for 2 hours. The obtained mixed powder is loaded into a stainless steel boat and placed in a sintering furnace for low-temperature sintering in a hydrogen atmosphere. The sintering parameters are: temperature 500°C, insulation time 1 hour; after sintering, the mixture is cooled with the furnace and taken out to obtain a sintered material; the obtained sintered material is crushed to 40-50 meshes using an ultrasonic vibrating screen machine to obtain a sintered powder;
[0027] 3) Take The pure copper tube is placed on a vibration platform (HZ-4006B vibration platform of Dongguan Lixian Instrument Technology Co., Ltd.), and the sintered powder obtained in step 2) is uniformly filled into the copper tube, and the filled powder is vibrated layer by layer under the vibration of the platform; the electrode blank after vibration is loaded into a vacuum furnace for vacuum sintering, and the sintering parameters are: vacuum reading ≤ 0.01Pa, sintering temperature 1000℃, and insulation time 2h; the excess copper tube after sintering shrinkage is cut off to obtain a dense and uniform copper-chromium 25 consumable electrode. After testing, the relative density of the obtained copper-chromium 25 consumable electrode is 71%.
[0028] The copper-chromium 25 consumable electrode prepared in this example was used for vacuum consumable arc melting at a melting voltage of 23 V and a melting current of 1800 A to obtain Ingot, production The copper-chromium 25 contact product has a yield rate of 92%. The metallographic structure of the copper-chromium 25 contact product is as follows: Figure 1 shown.
[0029] Comparative Example 1
[0030] Example 1 was repeated, except that in step 2), the operation of sintering the mixed powder at low temperature and crushing the sintered material was omitted, that is, the mixed powder obtained by mixing the weighed copper powder and chromium powder in a mixer for 2 hours was directly subjected to step 3) and subsequent steps. After testing, the relative density of the obtained copper-chromium 25 consumable electrode was 62%.
[0031] The copper-chromium 25 consumable electrode prepared in this comparative example was used for vacuum consumable arc melting at a melting voltage of 23 V and a melting current of 1800 A to obtain Ingot, production The copper-chromium 25 contact product has a yield rate of 70%. The metallographic structure of the copper-chromium 25 contact product is as follows: Figure 2 shown.
[0032] Example 2
[0033] 1) Weigh 40% copper powder and 60% chromium powder by weight and set aside;
[0034] 2) The weighed copper powder and chromium powder are placed in a mixer and mixed for 3 hours. The obtained mixed powder is loaded into a stainless steel boat and placed in a sintering furnace for low-temperature sintering in a hydrogen atmosphere. The sintering parameters are: temperature 350°C, insulation time 2 hours; after sintering, the mixture is cooled with the furnace and taken out to obtain a sintered material; the obtained sintered material is crushed to 50-60 meshes using an ultrasonic vibrating screen machine to obtain a sintered powder;
[0035] 3) Take The pure copper tube is placed on a vibration platform (HZ-4006B vibration platform, Dongguan Lixian Instrument Technology Co., Ltd.), and the sintered powder obtained in step 2) is uniformly filled into the copper tube, and the filled powder is vibrated layer by layer under the vibration of the platform; the electrode blank after vibration is loaded into a vacuum furnace for vacuum sintering, and the sintering parameters are: vacuum reading ≤0.01Pa, sintering temperature 900℃, and insulation time 6h; the excess copper tube after sintering shrinkage is cut off to obtain a dense and uniform composition. Copper-chromium 40 consumable electrode. After testing, the relative density of the obtained copper-chromium 40 consumable electrode is 74%.
[0036] The copper-chromium 40 consumable electrode prepared in this example was used for vacuum consumable arc melting at a melting voltage of 24 V and a melting current of 2300 A to obtain Ingot, production The copper-chromium 40 contact product has a yield rate of 94%. The metallographic structure of the copper-chromium 40 contact product is as follows: Figure 3 shown.
[0037] Comparative Example 2-1
[0038] Example 2 was repeated, except that in step 2), the sintering parameters were changed to: temperature 600° C., holding time 0.5 h. After testing, the relative density of the obtained copper-chromium 40 consumable electrode was 68%.
[0039] The copper-chromium 40 consumable electrode prepared in this comparative example was used for vacuum consumable arc melting at a melting voltage of 24 V and a melting current of 2300 A to obtain Ingot, production The copper-chromium 40 contact product has a yield rate of 79%. The metallographic structure of the copper-chromium 40 contact product is as follows: Figure 4 shown.
[0040] Comparative Example 2-2
[0041] Example 2 was repeated, except that in step 2), the sintering parameters were changed to: temperature 250° C., holding time 3 h. After testing, the relative density of the obtained copper-chromium 40 consumable electrode was 65%.
[0042] The copper-chromium 40 consumable electrode prepared in this comparative example was used for vacuum consumable arc melting at a melting voltage of 24 V and a melting current of 2300 A to obtain Ingot, production The copper-chromium 40 contact product has a yield rate of 73%. The metallographic structure of the copper-chromium 40 contact product is as follows: Figure 5 shown.
[0043] Example 3
[0044] 1) Weigh 45% copper powder and 55% chromium powder by weight and set aside;
[0045] 2) The weighed copper powder and chromium powder are placed in a mixer and mixed for 5 hours. The obtained mixed powder is loaded into a stainless steel boat and placed in a sintering furnace for low-temperature sintering in a hydrogen atmosphere. The sintering parameters are: temperature 400°C, insulation time 0.5h; after sintering, the mixture is cooled with the furnace and taken out to obtain a sintered material; the obtained sintered material is crushed to 40-50 meshes using an ultrasonic vibrating screen machine to obtain a sintered powder;
[0046] 3) Take The chromium bronze tube (TCr0.5 tube) is placed on a vibration platform (HZ-4006B vibration platform, Dongguan Lixian Instrument Technology Co., Ltd.), and the sintered powder obtained in step 2) is uniformly filled into the copper tube, and the filled powder is vibrated layer by layer under the vibration of the platform; the electrode blank after vibration is loaded into a vacuum furnace for vacuum sintering, and the sintering parameters are: vacuum reading ≤0.01Pa, sintering temperature 1050℃, and insulation time 1h; the excess chromium bronze tube after sintering shrinkage is cut off to obtain a dense and uniform composition. Copper-chromium 55 consumable electrode. After testing, the relative density of the obtained copper-chromium 55 consumable electrode is 72%.
[0047] The copper-chromium 55 consumable electrode prepared in this example was used for vacuum consumable arc melting at a melting voltage of 26 V and a melting current of 2400 A to obtain Ingot, production The copper-chromium 55 contact product has a yield rate of 93%. The metallographic structure of the copper-chromium 55 contact product is as follows: Figure 6 shown.
[0048] The gas content of the consumable electrodes prepared in the above-mentioned embodiments and comparative examples was tested, and the results are shown in the following Table 1.
[0049] Table 1:
[0050]
Claims
1. A method for preparing a copper-chromium consumable electrode, The following steps are involved: 1) Weigh the corresponding amount of copper powder and chromium powder according to the alloy composition required by the process and set aside; 2) The weighed copper powder and chromium powder are mixed evenly, the obtained mixed powder is sintered at low temperature in a reducing atmosphere, and the obtained sintered material is crushed to obtain a sintered powder; wherein the low temperature sintering is carried out at a temperature of 300 to 550° C.; 3) The obtained sintered powder is filled into a metal sheath, and after being vibrated, it is placed under vacuum conditions for vacuum sintering to obtain the copper-chromium consumable electrode.
2. The method according to claim 1, Its characteristics are: In step 2), the holding time of low temperature sintering is 0.5 to 2 hours.
3. The method according to claim 1, Its characteristics are: In step 2), the sintered material is crushed to a size less than or equal to 40 mesh.
4. The method according to any one of claims 1 to 3, Its characteristics are: In step 3), vacuum sintering is performed at 900-1050°C.
5. The method according to claim 4, Its characteristics are: In step 3), the holding time of vacuum sintering is greater than or equal to 1 hour.
6. The method according to claim 4, Its characteristics are: In step 3), the holding time of vacuum sintering is 1.5 to 6 hours.
7. The method according to any one of claims 1 to 3, Its characteristics are: In step 1), copper powder and chromium powder are weighed in weight percentages of 75-45% and 25-55%, respectively.