Electric heating paint, electric heating coating and preparation method and application thereof

By using additives and aqueous graphene in electric heating coatings, the near-field infrared thermal radiation efficiency is enhanced, and the problem of energy consumption of traditional electric heating coatings is solved, and an efficient and energy-saving deicing effect is achieved. It is suitable for electricity in wind power blades Heat to prevent ice covering and deicing.

CN119039853APending Publication Date: 2024-11-29STATE POWER INVESTMENT CORPORATION RESEARCH INSTITUTE +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411161074.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional electric thermal anti-icing coatings consume a lot of energy, resulting in low deicing efficiency of wind turbine blades in wet and cold areas, affecting power generation efficiency and equipment safety.

Method used

Use additives and aqueous graphene to enhance the near-field infrared thermal radiation efficiency of graphene, improve the heating rate and heating area of ​​the coating, and use bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide or antimony selenide as semiconductor additives , form a continuous conductive network composite structure to enhance the thermal radiation effect.

Benefits of technology

It significantly improves the deicing efficiency, reduces energy consumption, has high electric heat conversion efficiency, strong thermal radiation, and fast heating rate. It is suitable for electric heating of wind power blades to prevent ice covering and deicing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006426410000091
    Figure BDA0005006426410000091
Patent Text Reader

Abstract

The invention discloses an electrothermal coating, an electrothermal coating and a preparation method and application of the electrothermal coating and the electrothermal coating. 25 to 35 parts of water-based graphene; 40-60 parts of a curing agent; 10 to 15 parts of an auxiliary agent; 1 to 2 parts of a surfactant; wherein the auxiliary agent comprises at least one of bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide and antimony selenide. According to the electric heating coating, the auxiliaries and the water-based graphene are compounded and have a synergistic effect, so that the near-field infrared heat radiation efficiency of the graphene can be enhanced, the heating rate of the coating is increased, the heating area of the coating is expanded, and the deicing efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of deicing, and in particular to an electrothermal paint, an electrothermal coating, and a preparation method and application thereof. Background Art

[0002] Blades are one of the most critical components of wind turbines. Their appearance, structural characteristics and mechanical strength are directly related to the reliability and stability of the whole machine operation, and have an important impact on the power generation efficiency. Most wind turbines are installed in humid and cold areas, and their working environment is harsh, which can easily cause blades to freeze. Blade icing seriously affects the normal operation of the power system and causes power generation loss; it seriously affects the load and output of the wind turbine unit, reduces the design life of the unit, and the falling ice will cause safety hazards to surrounding equipment and personnel.

[0003] Electric thermal anti-icing / deicing has the advantages of high efficiency and flexible and convenient deicing methods, and is currently one of the important anti-icing / deicing methods in the wind power field. However, traditional electric thermal coatings used for electric thermal anti-icing / deicing generally have the problem of high energy consumption, so it is of great significance to find efficient and energy-saving electric thermal coatings. Summary of the invention

[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems: the current graphene electrothermal coating mainly transfers the heat generated by the graphene to the blade surface for de-icing in the form of heat conduction, and most of the heat only acts on the contact surface between the electrothermal coating and the ice layer.

[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the embodiments of the present invention provide an electric heating paint, an electric heating coating and a preparation method and application thereof, wherein the additive and the water-based graphene are compounded synergistically to enhance the near-field infrared thermal radiation efficiency of the graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the deicing efficiency.

[0006] The embodiment of the present invention provides an electrothermal coating, which comprises, by mass:

[0007] 100 parts of water-based resin;

[0008] 25-35 parts of water-based graphene;

[0009] 40-60 parts of curing agent;

[0010] 10-15 parts of additives;

[0011] 1-2 parts surfactant;

[0012] Wherein, the auxiliary agent includes at least one of bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide and antimony selenide.

[0013] Advantages and technical effects of the electric heating paint of the embodiment of the present invention: The electric heating paint uses semiconductor additives such as bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide or antimony selenide, and the additives are compounded with water-based graphene to synergistically enhance the near-field infrared thermal radiation efficiency of graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the deicing efficiency. The electric heating paint has high electrothermal conversion efficiency, strong thermal radiation, fast heating rate, high deicing efficiency, and high efficiency and energy saving.

[0014] In the embodiments of the present invention, near-field thermal radiation is a heat transfer phenomenon when the distance between objects is less than the wavelength of thermal radiation. Since the frequency band of graphene surface plasmons highly overlaps with the thermal radiation spectrum, it is of great advantage to enhance near-field thermal radiation by using the strong coupling of graphene surface plasmons at close distances. In addition to heat transfer in the form of thermal conduction, the thermal radiation effect of the electrothermal coating of the present invention is significantly enhanced. The heat from thermal conduction mainly acts on the contact surface between the coating and the ice layer. The thermal radiation heat of the electrothermal coating of the present invention can act on the entire ice layer. The thermal radiation can act within 20 cm from the coating surface, and ice layers with a thickness of less than 10 cm are within the radiation range of the coating.

[0015] In the embodiment of the present invention, the additives used in the present invention, bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide or antimony selenide, can realize the energy-free movement of electrons on their surfaces at low temperatures. After the additives are mixed with graphene, they work together to enhance the migration of graphene electrons, thereby enhancing the coupling of graphene surface plasmons at close range to enhance thermal radiation. In this process, the coating temperature rises, and the electrons migrate further under the influence of the temperature rise until the coating temperature is constant, the carrier migration rate is constant, and the thermal radiation effect is stable. Other semiconductor additives require energy to drive the electrons, and mixing with graphene will hinder the migration of graphene electrons and lattice vibration, and weaken thermal radiation and heat conduction.

[0016] In an embodiment of the present invention, when the electrothermal coating uses an additive but does not add water-based graphene, the coating does not generate heat. When the electrothermal coating uses water-based graphene but does not add an additive, the thermal radiation effect is weak, and the coating mainly transfers heat in the form of heat conduction, and the range of action on the ice layer is small. The additive and water-based graphene are compounded, and the continuous conductive network composite structure formed by the additive and the water-based graphene can further enhance the near-field thermal radiation, increase the range and intensity of action on the ice layer, and the coating has good heat generation and strong thermal radiation. The heat generated by the coating acts on the entire ice layer, thereby improving the deicing efficiency. By adding a surfactant, the compatibility of the additive and the water-based graphene can be improved. The electrothermal coating uses water-based graphene, and the water-based graphene is compounded with a water-based resin, with water as the dispersion medium. The two have good mutual dispersibility, low cost, and low pollution.

[0017] In some embodiments, the average particle size of the auxiliary agent is 40 to 60 μm.

[0018] In some embodiments, the solid content of the aqueous graphene is 25-40%.

[0019] In some embodiments, the water-based resin includes water-based epoxy resin and / or water-based polyurethane; optionally, the water-based epoxy resin includes at least one of bisphenol A epoxy resin E51, acrylic epoxy resin, glycerol epoxy resin, and alicyclic epoxy resin.

[0020] In some embodiments, the curing agent includes at least one of triethylenetetramine, diaminodiphenylmethane, isophoronediamine, polyether polyol, polyester polyol, and polyolefin polyol.

[0021] In some embodiments, the surfactant includes at least one of sodium dodecyl sulfate, sodium fatty alcohol polyoxyethylene ether sulfate, and fatty alcohol polyoxyethylene ether.

[0022] In some embodiments, the viscosity of the electrothermal paint is 800-1500 cP.

[0023] An embodiment of the present invention provides a method for preparing an electrothermal coating, comprising the following steps:

[0024] (1) mixing water-based graphene, an auxiliary agent and a surfactant to obtain a mixed dispersion;

[0025] (2) mixing the mixed dispersion with an aqueous resin to obtain a mixed slurry;

[0026] (3) The mixed slurry is mixed with a curing agent to obtain an electric heating paint.

[0027] In the embodiment of the present invention, an auxiliary agent and a surfactant are first added to the water-based graphene, which is conducive to the full mixing of the water-based graphene and the auxiliary agent, and improves the enhancing effect of the auxiliary agent on the near-field thermal radiation of the water-based graphene; then the resin is added for mixing, and the mixed dispersion and the resin are evenly dispersed, which is conducive to the uniformity of heat generation after the coating is cured; finally, the curing agent is added and mixed to obtain the electric heating coating.

[0028] An embodiment of the present invention provides an electrothermal coating, which is obtained by curing an electrothermal coating. The electrothermal coating includes the electrothermal coating described in the embodiment of the present invention or the electrothermal coating obtained by the preparation method described in the embodiment of the present invention, and a heating electrode is provided in the electrothermal coating.

[0029] In the embodiment of the present invention, the additive and the water-based graphene are compounded synergistically to enhance the near-field infrared thermal radiation efficiency of the graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the deicing efficiency.

[0030] In some embodiments, the heating electrode includes a positive electrode and a negative electrode, and the electrode spacing between the positive electrode and the negative electrode is 6 to 10 cm;

[0031] And / or, the electrode is copper foil;

[0032] And / or, the thickness of the electrothermal coating is 100-350 μm.

[0033] The embodiment of the present invention provides a method for preparing an electrothermal coating, comprising: arranging a heating electrode on a substrate, then coating an electrothermal coating on the substrate after the heating electrode is arranged, and curing the coating to obtain the electrothermal coating.

[0034] The embodiment of the present invention provides an application of an electrothermal paint or electrothermal coating for electric heating of wind turbine blades to prevent ice and / or de-ice. In the embodiment of the present invention, the additive and the water-based graphene are compounded synergistically to enhance the near-field infrared thermal radiation efficiency of the graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the de-icing efficiency of the wind turbine blades.

[0035] In some embodiments, the time taken by the electrothermal coating to remove ice layers with a thickness of less than 10 cm is no longer than 60 minutes. DETAILED DESCRIPTION

[0036] Embodiments of the present invention are described in detail below. The embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0037] An electrothermal coating according to an embodiment of the present invention comprises, by mass:

[0038] 100 parts of water-based resin;

[0039] 25-35 parts of water-based graphene;

[0040] 40-60 parts of curing agent;

[0041] 10-15 parts of additives;

[0042] 1-2 parts surfactant;

[0043] Wherein, the auxiliary agent includes at least one of bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide and antimony selenide.

[0044] The electric heating paint of the embodiment of the present invention adopts semiconductor additives such as bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide or antimony selenide, and the additives are compounded with water-based graphene to synergistically enhance the near-field infrared thermal radiation efficiency of graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the deicing efficiency. The electric heating paint has high electrothermal conversion efficiency, strong thermal radiation, fast heating rate, high deicing efficiency, and high efficiency and energy saving.

[0045] In the embodiments of the present invention, near-field thermal radiation is a heat transfer phenomenon when the distance between objects is less than the wavelength of thermal radiation. Since the frequency band of graphene surface plasmons highly overlaps with the thermal radiation spectrum, it is of great advantage to enhance near-field thermal radiation by using the strong coupling of graphene surface plasmons at close distances. In addition to heat transfer in the form of thermal conduction, the thermal radiation effect of the electrothermal coating of the present invention is significantly enhanced. The heat from thermal conduction mainly acts on the contact surface between the coating and the ice layer. The thermal radiation heat of the electrothermal coating of the present invention can act on the entire ice layer. The thermal radiation can act within 20 cm from the coating surface, and ice layers with a thickness of less than 10 cm are within the radiation range of the coating.

[0046] In the embodiment of the present invention, the additives used in the present invention, bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide or antimony selenide, can realize the energy-free movement of electrons on their surfaces at low temperatures. After the additives are mixed with graphene, they work together to enhance the migration of graphene electrons, thereby enhancing the coupling of graphene surface plasmons at close range to enhance thermal radiation. In this process, the coating temperature rises, and the electrons migrate further under the influence of the temperature rise until the coating temperature is constant, the carrier migration rate is constant, and the thermal radiation effect is stable. Other semiconductor additives require energy to drive the electrons, and mixing with graphene will hinder the migration of graphene electrons and lattice vibration, and weaken thermal radiation and heat conduction.

[0047] In an embodiment of the present invention, when the electrothermal coating uses an additive but does not add water-based graphene, the coating does not generate heat. When the electrothermal coating uses water-based graphene but does not add an additive, the thermal radiation effect is weak, and the coating mainly transfers heat in the form of heat conduction, and the range of action on the ice layer is small. The additive and water-based graphene are compounded, and the continuous conductive network composite structure formed by the additive and the water-based graphene can further enhance the near-field thermal radiation, increase the range and intensity of action on the ice layer, and the coating has good heat generation and strong thermal radiation. The heat generated by the coating acts on the entire ice layer, thereby improving the deicing efficiency. By adding a surfactant, the compatibility of the additive and the water-based graphene can be improved. The electrothermal coating uses water-based graphene, and the water-based graphene is compounded with a water-based resin, with water as the dispersion medium. The two have good mutual dispersibility, low cost, and low pollution.

[0048] In some embodiments, the electrothermal coating includes 10 to 15 parts of additives by mass, specifically, for example, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, and 15 parts. In the embodiment of the present invention, the additive is preferably 10 to 15 parts, and the additive can form a continuous conductive network composite structure with the water-based graphene, significantly enhancing thermal radiation. When the additive content is too low, for example, 1 part, the additive is dispersed in the water-based graphene, and the distance between them is far, and the coupling of the graphene surface plasmons cannot be effectively enhanced, and the thermal radiation enhancement effect is relatively unobvious; when the additive content is too high, the excess additive particles hinder the electron migration of the water-based graphene, affecting the coupling of the plasmons, resulting in weakened thermal radiation.

[0049] In some embodiments, the average particle size of the auxiliary agent is 40 to 60 μm, specifically, for example, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm. In the embodiment of the present invention, the average particle size of the auxiliary agent is 40 to 60 μm, which can be evenly dispersed with graphene to form a continuous conductive network composite structure. When the average particle size of the auxiliary agent is too small, it is easy to agglomerate and difficult to disperse; when the average particle size of the auxiliary agent is too large, it has poor compatibility with water-based graphene and poor dispersibility.

[0050] In some embodiments, the electrothermal coating includes 25 to 35 parts of water-based graphene, specifically, for example, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts; the solid content of the water-based graphene is 25 to 40%, specifically, for example, 25%, 30%, 35%, 40%; the dispersion concentration of the water-based graphene in water changes by no more than 5% within 10 days. In an embodiment of the present invention, the electrothermal coating includes water-based graphene materials, and graphene, resin and additives are blended with water as a dispersion system, which has strong dispersibility and is green and environmentally friendly. By preferably using 25 to 35 parts of water-based graphene, a continuous conductive network structure can be formed in the resin, giving the resin coating excellent electrothermal properties. When the content of water-based graphene is too low, a conductive network cannot be formed in the resin; when the content of water-based graphene is too high, the resin curing structure is destroyed, the coating is difficult to cure and form, and the physical properties are weak.

[0051] In some embodiments, the electrothermal coating includes 1 to 2 parts of a surfactant, specifically, for example, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts; optionally, the surfactant includes at least one of sodium dodecyl sulfonate, sodium sulfate of fatty alcohol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether. In an embodiment of the present invention, the compatibility of the auxiliary agent with water-based graphene can be enhanced by adding a surfactant. When the surfactant content is too high, the conductive network composite structure formed by the auxiliary agent and the water-based graphene may be destroyed. The surfactant sodium dodecyl sulfonate, sodium sulfate of fatty alcohol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether can effectively enhance the compatibility of the auxiliary agent with water-based graphene.

[0052] In some embodiments, the water-based resin includes water-based epoxy resin and / or water-based polyurethane; optionally, the water-based epoxy resin includes at least one of bisphenol A epoxy resin E51, acrylic epoxy resin, glycerol epoxy resin, and alicyclic epoxy resin; optionally, the solid content of the water-based resin is 40% to 60%, specifically, for example, 40%, 45%, 50%, 55%, 60%; optionally, the solid content of the water-based epoxy resin is 40% to 60%, specifically, for example, 40%, 45%, 50%, 55%, 60%.

[0053] In some embodiments, the electrothermal coating includes 40 to 60 parts of a curing agent, specifically, for example, 40 parts, 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, 50 parts, 55 parts, and 60 parts; the curing agent includes at least one of triethylenetetramine, diaminodiphenylmethane, isophoronediamine, polyether polyol, polyester polyol, and polyolefin polyol.

[0054] In some embodiments, the electrothermal coating further comprises water; preferably, the electrothermal coating, by mass, further comprises 20 to 50 parts of water, specifically, for example, 20 parts, 30 parts, 40 parts, 45 parts, 50 parts. In the embodiment of the present invention, both the water-based resin and the water-based graphene contain water, and water may not be added to the coating, or an appropriate amount of water may be added according to the viscosity adjustment requirements of the coating.

[0055] In some embodiments, the viscosity of the electrothermal paint is 800-1500 cP, specifically, for example, 800 cP, 900 cP, 1000 cP, 1100 cP, 1200 cP, 1300 cP, 1400 cP, 1500 cP. In the embodiments of the present invention, the viscosity of the electrothermal paint is 800-1500 cP, which is conducive to the uniform mixing of the components of the electrothermal paint; if the viscosity is too high, the components are unevenly dispersed; if the viscosity is too low, the electrothermal paint is difficult to apply.

[0056] A method for preparing an electrothermal coating according to an embodiment of the present invention comprises the following steps:

[0057] (1) mixing water-based graphene, an auxiliary agent and a surfactant to obtain a mixed dispersion;

[0058] (2) mixing the mixed dispersion with an aqueous resin to obtain a mixed slurry;

[0059] (3) The mixed slurry is mixed with a curing agent to obtain an electric heating paint.

[0060] In the embodiment of the present invention, an auxiliary agent and a surfactant are first added to the water-based graphene, which is conducive to the full mixing of the water-based graphene and the auxiliary agent, and improves the enhancing effect of the auxiliary agent on the near-field thermal radiation of the water-based graphene; then the resin is added for mixing, and the mixed dispersion and the resin are evenly dispersed, which is conducive to the uniformity of heat generation after the coating is cured; finally, the curing agent is added and mixed to obtain the electric heating coating.

[0061] In some embodiments, in step (1), stirring is performed after mixing, and the stirring time is 5 to 10 minutes.

[0062] In some embodiments, in step (2), stirring is performed after mixing, and the stirring time is 10 to 15 minutes.

[0063] In some embodiments, in step (3), stirring is performed after mixing, and the stirring time is 5 to 10 minutes.

[0064] In some embodiments, the electrothermal coating further comprises water. In the step (1), the water-based graphene, the additive, the surfactant and the water are mixed to obtain a mixed dispersion.

[0065] An electrothermal coating according to an embodiment of the present invention is obtained by curing an electrothermal coating. The electrothermal coating includes the electrothermal coating according to the embodiment of the present invention or the electrothermal coating obtained by the preparation method according to the embodiment of the present invention. A heating electrode is provided in the electrothermal coating.

[0066] In the embodiment of the present invention, the additive and the water-based graphene are compounded synergistically to enhance the near-field infrared thermal radiation efficiency of the graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the deicing efficiency.

[0067] In some embodiments, the heating electrode includes a positive electrode and a negative electrode, and the electrode spacing between the positive electrode and the negative electrode is 6 to 10 cm, specifically, for example, 6 cm, 7 cm, 8 cm, 9 cm, 10 cm; and / or, the electrode is a copper foil; optionally, the copper foil is 0.1 mm thick × 5 mm wide. In the embodiment of the present invention, the electrode spacing of 6 to 10 cm is conducive to the coating having the best electrothermal performance while maintaining a stable structure. When the electrode spacing is too small, the electron migration rate of the coating is too large, which is easy to damage the internal structure of the coating; when the electrode spacing is too large, it is difficult for electrons to migrate.

[0068] In some embodiments, the thickness of the electrothermal coating is 100 to 350 μm, specifically, for example, 100 μm, 200 μm, 300 μm, 350 μm. In the embodiment of the present invention, the thickness of the electrothermal coating is preferably 100 to 350 μm, which is conducive to obtaining an electrothermal coating with excellent electrothermal performance. When the electrothermal coating is too thin, the number of carriers accommodated is relatively small, the electrothermal performance is weak, and it is easy to be damaged; when the electrothermal coating is too thick, the blade load is increased, the operation of the blade is affected, and the construction difficulty and cost are increased.

[0069] A method for preparing an electrothermal coating according to an embodiment of the present invention comprises: arranging a heating electrode on a substrate, then coating an electrothermal coating on the substrate on which the heating electrode is arranged, and curing the coating to obtain the electrothermal coating.

[0070] In some embodiments, the curing temperature is 5 to 60°C, specifically, for example, 5°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C.

[0071] In some embodiments, the coating is performed by spraying.

[0072] An application of an electrothermal paint or electrothermal coating according to an embodiment of the present invention is used for electric heating of wind turbine blades to prevent ice and / or de-ice. In an embodiment of the present invention, the additive and water-based graphene are compounded to synergistically enhance the near-field infrared thermal radiation efficiency of graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the de-icing efficiency of wind turbine blades.

[0073] In some embodiments, the electrothermal coating takes no longer than 60 minutes to remove an ice layer less than 10 cm thick; specifically, under the conditions of 120V power and an ambient temperature of -5 to -2°C, the electrothermal coating takes no longer than 60 minutes to remove an ice layer less than 10 cm thick, specifically, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, or 60 minutes.

[0074] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0075] Example 1

[0076] A method for preparing an electrothermal coating comprises the following steps:

[0077] (1) By mass, 10 g of bismuth sulfide (40-60 μm) and 2 g of sodium dodecyl sulfate were added to 30 g of aqueous graphene (solid content of 25-40%) and stirred for 8 min to obtain a mixed dispersion.

[0078] (2) By mass, the mixed dispersion of step (1) was added to 100 g of water-based bisphenol A epoxy resin E51 (solid content 40% to 60%), and the mixture was stirred for 15 min. Then, 50 g of triethylenetetramine was added and stirred for 8 min to obtain an electric heating coating. The viscosity of the coating was measured to be 800 to 1500 cP.

[0079] (3) Preparation of electric heating coating: heating electrodes (electrode spacing 8 cm) were arranged on the substrate, and the electric heating coating was applied by spraying. The coating was cured at 25°C. After complete curing, the electric heating coating was obtained. The thickness of the electric heating coating was about 350 μm.

[0080] Example 2

[0081] The preparation method is the same as that of Example 1, except that in step (1), the amount of bismuth sulfide added is 13 g.

[0082] Example 3

[0083] The preparation method is the same as that of Example 1, except that in step (1), the amount of bismuth sulfide added is 15 g.

[0084] Example 4

[0085] The preparation method is the same as that of Example 1, except that in step (1), bismuth sulfide (40-60 μm) is replaced by antimony selenide (40-60 μm).

[0086] Example 5

[0087] The preparation method is the same as that of Example 1, except that in step (1), bismuth sulfide (40-60 μm) is replaced by lead sulfide (40-60 μm).

[0088] Example 6

[0089] The preparation method is the same as that of Example 1, except that in step (1), bismuth sulfide (40-60 μm) is replaced by cadmium sulfide (40-60 μm).

[0090] Example 7

[0091] The preparation method is the same as that of Example 1, except that in step (1), bismuth sulfide (40-60 μm) is replaced by 5 g of antimony selenide (40-60 μm) and 5 g of bismuth telluride (40-60 μm).

[0092] Example 8

[0093] The preparation method is the same as that in Example 1, except that the amount of water-based graphene is 35 g.

[0094] Example 9

[0095] The preparation method is the same as that in Example 1, except that the amount of water-based graphene is 25 g.

[0096] Comparative Example 1

[0097] The preparation method is the same as that of Example 1, except that in step (1), bismuth sulfide and sodium dodecyl sulfate are not added to the aqueous graphene.

[0098] Comparative Example 2

[0099] The preparation method is the same as that of Example 1, except that in step (1), the amount of bismuth sulfide added is 17 g.

[0100] Comparative Example 3

[0101] The preparation method is the same as that of Example 1, except that in step (1), the amount of bismuth sulfide added is 20 g.

[0102] Comparative Example 4

[0103] The preparation method is the same as that of Example 1, except that in step (1), bismuth sulfide is replaced by semiconductor material silicon carbide (40-60 μm).

[0104] Comparative Example 5

[0105] The preparation method is the same as that of Example 1, except that in step (1), the amount of water-based graphene used is 10 g.

[0106] Comparative Example 6

[0107] The preparation method is the same as that of Example 1, except that in step (1), the amount of water-based graphene used is 50 g.

[0108] Comparative Example 7

[0109] The preparation method is the same as that of Example 1, except that in step (1), the water-based graphene is replaced with graphene powder of equal graphene mass, and the graphene powder, bismuth sulfide, sodium dodecyl sulfate and 30g water are mixed and stirred for 8min to obtain a mixed dispersion. In step (3), the electric heating coating is applied by scraping.

[0110] Comparative Example 8

[0111] The preparation method is the same as that in Example 1, except that in the step (1), the aqueous graphene is replaced with graphene oxide powder having an equal mass of graphene, and the graphene oxide powder, bismuth sulfide, sodium dodecyl sulfate and 30 g of water are mixed and stirred for 8 min to obtain a mixed dispersion.

[0112] Comparative Example 9

[0113] The preparation method is the same as that of Example 1, except that the electrode spacing is 4 cm.

[0114] Comparative Example 10

[0115] The preparation method is the same as that of Example 1, except that the electrode spacing is 12 cm.

[0116] Comparative Example 11

[0117] The preparation method is the same as that of Comparative Example 1, except that the thickness of the electrothermal coating is 50 μm.

[0118] The electrothermal performance and deicing performance tests were carried out on the electrothermal coating: the coating surface heating rate was tested under room temperature conditions with a power supply of 120V; the coating was tested for the time required to remove 3 to 10 cm of ice on the surface of the wind turbine blade under conditions of a power supply of 120V and an ambient temperature of -5 to -2°C.

[0119] Table 1

[0120]

[0121] It can be seen from Table 1 that the electrothermal performance and deicing efficiency of the electrothermal coatings in Examples 1 to 9 are relatively good, the heating rate is higher than 40° C. / min, and the deicing time is no longer than 60 min.

[0122] The electric heating coating in Comparative Example 1 does not have the additive bismuth sulfide added, the thermal radiation of the coating is not enhanced, the electric heating performance is relatively weak, and the deicing efficiency is low.

[0123] The auxiliary agent bismuth sulfide content in Comparative Examples 2 and 3 is too high, which affects the formation of a conductive network by the water-based graphene in the polymer matrix of the coating, hinders the electron migration of the water-based graphene, causes the thermal radiation to be weakened, and the electrothermal performance of the coating is weakened.

[0124] In Comparative Example 4, silicon carbide is used as an auxiliary agent, and silicon carbide hinders the migration of electrons in water-based graphene, causing the coating to lose its electrothermal properties.

[0125] The amount of water-based graphene added to the coating of Comparative Example 5 is too small, and the water-based graphene does not form a conductive network in the system, resulting in the coating having no electrothermal properties.

[0126] The amount of water-based graphene added to the electric heating coating of Comparative Example 6 is too much, which affects the curing of the water-based resin and makes the coating difficult to form.

[0127] The electric heating coating of comparative example 7 uses graphene powder blended with resin, the graphene powder has poor dispersibility, and the electric heating performance and deicing performance of the electric heating coating are relatively poor.

[0128] The electric heating coating of Comparative Example 8 uses graphene oxide powder. Graphene oxide contains more oxygen-containing groups and has weaker conductivity than water-based graphene. The electric heating coating prepared by replacing water-based graphene with graphene oxide has weaker electric heating performance and reduced deicing efficiency.

[0129] In the electrothermal coating of Comparative Example 9, the distance between electrodes is too small, and the driving force of the electrons inside the coating due to the external electric field can easily lead to damage to the coating structure.

[0130] The thickness of the electric heating coating in Comparative Example 11 is too thin, the number of carriers under the same voltage driving is small, the thermal radiation is weakened, and the deicing efficiency is reduced.

[0131] In summary, adding water-based graphene and additives such as bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide, and antimony selenide to the electric heating coating, and the synergistic effect of the additives and water-based graphene can enhance the near-field infrared thermal radiation efficiency of graphene, increase the heating rate of the coating, expand the heating area of ​​the coating, and improve the deicing efficiency. The electric heating coating has excellent electrothermal characteristics and deicing performance.

[0132] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0133] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. An electrothermal coating, It is characterized in that In terms of quality, it includes: 100 parts of water-based resin; 25-35 parts of water-based graphene; 40-60 parts of curing agent; 10-15 parts of additives; 1-2 parts surfactant; Wherein, the auxiliary agent includes at least one of bismuth telluride, bismuth sulfide, lead sulfide, cadmium sulfide and antimony selenide.

2. The electrothermal paint according to claim 1, It is characterized in that The average particle size of the auxiliary agent is 40 to 60 μm; And / or, the solid content of the aqueous graphene is 25-40%.

3. The electrothermal paint according to claim 1, It is characterized in that The water-based resin includes water-based epoxy resin and / or water-based polyurethane; the water-based epoxy resin includes at least one of bisphenol A epoxy resin E51, acrylic epoxy resin, glycerol epoxy resin, and alicyclic epoxy resin; And / or, the curing agent includes at least one of triethylenetetramine, diaminodiphenylmethane, isophoronediamine, polyether polyol, polyester polyol, and polyolefin polyol; And / or, the surfactant includes at least one of sodium dodecyl sulfate, sodium fatty alcohol polyoxyethylene ether sulfate, and fatty alcohol polyoxyethylene ether.

4. The electrothermal paint according to claim 1, It is characterized in that The viscosity of the electrothermal paint is 800-1500 cP.

5. A method for preparing the electrothermal coating according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) mixing water-based graphene, an auxiliary agent and a surfactant to obtain a mixed dispersion; (2) mixing the mixed dispersion with an aqueous resin to obtain a mixed slurry; (3) The mixed slurry is mixed with a curing agent to obtain an electric heating paint.

6. An electric heating coating, It is characterized in that The electrothermal coating is obtained by curing an electrothermal paint, wherein the electrothermal paint includes the electrothermal paint described in any one of claims 1 to 4 or the electrothermal paint obtained by the preparation method described in claim 5, and a heating electrode is provided in the electrothermal coating.

7. The electric heating coating according to claim 6, It is characterized in that The heating electrode comprises a positive electrode and a negative electrode, and the electrode spacing between the positive electrode and the negative electrode is 6 to 10 cm; And / or, the electrode is copper foil; And / or, the thickness of the electrothermal coating is 100-350 μm.

8. A method for preparing the electrothermal coating according to claim 6 or 7, It is characterized in that include: A heating electrode is arranged on the substrate, and then an electric heating paint is coated on the substrate with the heating electrode arranged, and then cured to obtain an electric heating coating.

9. Use of the electrothermal paint according to any one of claims 1 to 4 or the electrothermal coating according to claim 6 or 7, It is characterized in that Used for electric heating of wind turbine blades to prevent icing and / or de-icing.

10. The use according to claim 9, It is characterized in that The time taken by the electric heating coating to remove ice layers less than 10 cm thick is no longer than 60 minutes.

Citation Information

Patent Citations

  • Super-hydrophobic anti-fouling anti-icing water-based paint

    CN112724830A

  • Solar power generation coating with anti-corrosion function as well as preparation method and application of solar power generation coating

    CN115975443A

  • Water-based weather-resistant antibacterial coiled material coating and preparation method thereof

    CN116751505A

  • Epoxy resin paint, epoxy resin coating and preparation method and application thereof

    CN117551380A

  • Preparation method of bismuth telluride thermoelectric material containing graphene

    CN117794344A