Nanoscale visible light emitting diode and preparation method thereof
By using dry etching in the Group III nitride light-emitting diode to form the nano-column array template and grow the active region, the piezoelectric polarization field problems caused by lattice mismatch and stress are solved, and the luminescence efficiency and wavelength control are improved. A highly efficient nanoscale visible light emitting diode is realized.
Patent Information
- Application Number
- CN202411153433.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The piezoelectric polarization field caused by lattice mismatch and stress during material growth process leads to a decrease in luminous efficiency, and the defect recombination under the nanometer size is severely affected, making it difficult to accurately control the luminous wavelength.
Two dry etching treatments were used to form a patterned Group III nitride semiconductor nanopillar array template, and the active region was grown sequentially on it. By reducing the impact of the quantum restricted Stark effect, it improved radiation recombination efficiency.
It realizes the improvement of the luminous intensity and external quantum efficiency of the light emitting diode at the nanoscale, reduces the energy required for In incorporation, enhances the incorporation of In content, extends the luminous wavelength, and effectively extracts photons, improving the light extraction efficiency .
Smart Images

Figure CN119050210A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor devices, and in particular relates to a nanometer-scale visible light emitting diode and a preparation method thereof. Background Art
[0002] III-nitride light-emitting diodes (LEDs) originated in the early 1990s, initially focusing on blue LEDs, and gradually developed into fields such as violet LEDs and white LEDs. With the development and maturity of technology, III-nitride LEDs have been widely used in display, lighting, communications and other fields, becoming a high-efficiency, environmentally friendly lighting and display technology.
[0003] During the material growth process, the optical bandgap width of group III nitride can be continuously adjusted from the infrared band to the ultraviolet band by adjusting the composition ratio of In / Ga / Al. Therefore, this material can be used to manufacture semiconductor optoelectronic devices from near-infrared to visible light and ultraviolet bands. Among them, the indium gallium nitride (InGaN) / gallium nitride (GaN) quantum well LED has high internal quantum efficiency and the emission wavelength covers the visible light band. It is a key structure for optoelectronic devices such as LEDs, laser diodes and photodetectors. Since the lattice constant of InGaN is greater than that of GaN, the InGaN quantum well is subjected to strong compressive strain, and as the In content increases, the strong compressive strain of the InGaN quantum well increases. The incorporation efficiency of In in InGaN is related to the strain energy required for the combination of the In-N bond. When the InGaN quantum well has strong compressive strain, the incorporation of In will be more difficult due to the need for higher strain energy. Therefore, it is difficult for the InGaN quantum well to reach a high In content and it is difficult to control the emission wavelength in a large range.
[0004] The strong compressive strain on the InGaN quantum well leads to the existence of a piezoelectric polarization field in the InGaN quantum well. The existence of this piezoelectric field will lead to the tilt of the energy band, causing the separation of the spatial distribution of the electron-hole wave function, resulting in a decrease in the probability of carrier radiation recombination and a red shift of the luminescence peak. This is called the quantum confined Stark effect, which will aggravate Auger recombination and electron leakage, reduce the electro-optical conversion efficiency of the active region, and is one of the key factors that hinder the improvement of the device's luminous efficiency. In addition, the refractive index difference between GaN and air causes some of the photons emitted in the quantum well to be totally reflected on the surface, and eventually absorbed and converted into heat energy, increasing the device temperature and further reducing the efficiency of the LED.
[0005] On the other hand, studies have shown that as the size of LEDs shrinks, they are more seriously affected by defect recombination, which often originates from the damage to the sidewall surface caused by etching the LED epitaxial wafer. Due to carrier diffusion and high sidewall surface state density, there is serious non-radiative recombination in the sidewall region, which reduces the LED luminous efficiency. Moreover, the InGaN active region after etching will undergo varying degrees of random stress relaxation. Due to the quantum confined Stark effect, the emission wavelength will shift after etching and is difficult to accurately control, and the device characteristics are highly random. Summary of the invention
[0006] In order to solve the problems caused by lattice mismatch and stress in the above-mentioned prior art, the present invention provides a nanoscale visible light emitting diode and a method for preparing the same. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0007] The embodiment of the present invention provides a method for preparing a nanoscale visible light emitting diode, comprising the steps of:
[0008] S1, growing a III-nitride semiconductor epitaxial layer on a substrate;
[0009] S2, depositing a first etching mask layer on the III-nitride semiconductor epitaxial layer;
[0010] S3, preparing a glue layer having a periodically arranged pattern on the first etching mask layer;
[0011] S4, depositing a mask material on the glue layer and in the periodic arrangement pattern, and stripping the mask material on the surface of the glue layer to form a patterned second etching mask layer on the first etching mask layer;
[0012] S5, dry-etching the first etch mask layer until the surface of the III-nitride semiconductor epitaxial layer in the area not covered by the patterned second etch mask layer is exposed, so that the pattern of the second etch mask layer is transferred to the first etch mask layer, and removing the patterned second etch mask layer to form a patterned first etch mask layer;
[0013] S6, dry-etching the III-nitride semiconductor epitaxial layer not covered by the patterned first etching mask layer, so that the pattern of the patterned first etching mask layer is transferred to the III-nitride semiconductor epitaxial layer, and removing the patterned first etching mask layer to form a III-nitride semiconductor current spreading layer and a patterned III-nitride semiconductor nanocolumn array template;
[0014] S7. Growing a first doping type III nitride semiconductor layer, an active region, and a second doping type III nitride semiconductor layer on the III nitride semiconductor nanocolumn array template from bottom to top in sequence to obtain a nanoscale visible light emitting diode, wherein the active region includes a quantum confinement layer, and the material of the quantum confinement layer includes an In-containing III nitride semiconductor.
[0015] In one embodiment of the present invention, step S1 comprises:
[0016] Growing a GaN nucleation layer, an unintentionally doped GaN layer, and a doped GaN layer on the substrate in sequence to form the III-nitride semiconductor epitaxial layer;
[0017] The doping type of the intentionally doped GaN layer includes n-type doping or p-type doping.
[0018] In one embodiment of the present invention, a ratio of the thickness of the first etch mask layer to the etching rate is smaller than a ratio of the thickness of the second etch mask layer to the etching rate.
[0019] In one embodiment of the present invention, the adhesive layer includes ultraviolet photoresist, electron beam photoresist or nano-imprinting adhesive.
[0020] In one embodiment of the present invention, the height of the nanocolumns in the III-nitride semiconductor nanocolumn array template is 100 nm to 5000 nm, the diameter of the nanocolumns is 50 nm to 1000 nm, and the distance between adjacent nanocolumns is 30 nm to 5000 nm.
[0021] In one embodiment of the present invention, before step S7, the method further includes:
[0022] The group III nitride semiconductor nano-column array template is immersed in an alkaline solution to etch the nano-columns with inclined side walls into nano-columns with vertical side walls.
[0023] In one embodiment of the present invention, the first doping type includes n-type, and the second doping type includes p-type, or the first doping type includes p-type, and the second doping type includes n-type;
[0024] The Ga contents of the first doping type III-nitride semiconductor layer and the second doping type III-nitride semiconductor layer are both not less than 70%.
[0025] In one embodiment of the present invention, the active region includes a plurality of quantum confinement layers, a plurality of barrier layers and an electron blocking layer, wherein:
[0026] The plurality of quantum confinement layers and the plurality of barrier layers are alternately stacked, and the quantum confinement layer is arranged between two adjacent barrier layers;
[0027] The electron blocking layer is arranged on the upper surface of the top barrier layer, or the electron blocking layer is arranged on the lower surface of the bottom barrier layer;
[0028] The quantum confinement layer can emit visible light with a wavelength of 380 to 780 nm under external excitation.
[0029] In one embodiment of the present invention, the active region includes a stress adjustment layer, a quantum confinement layer, a barrier layer and an electron blocking layer, wherein:
[0030] The quantum confinement layers and the barrier layers are alternately stacked, and the quantum confinement layer is arranged between two adjacent barrier layers;
[0031] The stress adjustment layer is arranged on the lower surface of the bottom barrier layer, and the electron blocking layer is arranged on the upper surface of the top barrier layer, or the electron blocking layer and the stress adjustment layer are stacked on the lower surface of the bottom barrier layer from top to bottom;
[0032] The quantum confinement layer can emit visible light with a wavelength of 380 to 780 nm under external excitation.
[0033] Another embodiment of the present invention provides a nanoscale visible light emitting diode, which is prepared by the preparation method described in the above embodiment, comprising: a group III nitride semiconductor current spreading layer, a patterned group III nitride semiconductor nanocolumn array template, a first doping type group III nitride semiconductor layer, an active region and a second doping type group III nitride semiconductor layer, wherein:
[0034] The nanocolumn array in the patterned III-nitride semiconductor nanocolumn array template is arranged on the III-nitride semiconductor current spreading layer and presents a periodic arrangement;
[0035] A first doping type III-nitride semiconductor layer, an active region, and a second doping type III-nitride semiconductor layer are sequentially stacked from bottom to top on each nanocolumn.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1. The present invention uses a first etching mask layer and a second etching mask layer to perform two dry etching processes to transfer a periodically arranged pattern to a III-nitride semiconductor epitaxial layer to form a patterned III-nitride semiconductor nanocolumn array template. The larger specific surface area of the nanocolumns can partially relax the strong compressive strain on the growing active region, which can reduce the energy required for In incorporation and effectively increase the incorporation of In in the In-containing quantum confinement layer, thereby achieving long-wavelength light emission; at the same time, since the strong compressive strain on the active region is partially relaxed, the piezoelectric polarization field in the In-containing quantum confinement layer is weakened, thereby effectively reducing the influence of the quantum confined Stark effect on the energy band, improving the radiation recombination efficiency, and increasing the luminous intensity of the light-emitting diode;
[0038] 2. The nanoscale visible light emitting diode of the present invention has a three-dimensional structure, and the sidewalls can effectively extract light, which is beneficial to improving the light extraction efficiency, thereby improving the external quantum efficiency of the light emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 A schematic flow chart of a method for preparing a nanoscale visible light emitting diode provided by an embodiment of the present invention;
[0040] Figure 2a-2f A schematic diagram of a process for preparing a nanoscale visible light emitting diode provided by an embodiment of the present invention;
[0041] Figure 3 This is a comparison chart of the luminescence spectrum of a nanoscale visible light emitting diode prepared by the preparation method of an embodiment of the present invention and the luminescence spectrum of a light emitting diode obtained by using a traditional planar template. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.
[0043] Embodiment 1
[0044] See also Figure 1 and Figure 2a-2f , Figure 1 A schematic diagram of a process for preparing a nanoscale visible light emitting diode provided by an embodiment of the present invention, Figure 2a-2f A schematic diagram of a process for preparing a nanoscale visible light emitting diode provided by an embodiment of the present invention. The method for preparing a nanoscale visible light emitting diode comprises the following steps:
[0045] S1. Growing a III-nitride semiconductor epitaxial layer B on a substrate A, such as Figure 2a shown.
[0046] Specifically, a GaN nucleation layer, an unintentionally doped GaN layer, and an intentionally doped GaN layer are sequentially grown from bottom to top on the surface of substrate A by using a metal organic chemical vapor deposition (MOCVD) process to form a III-nitride semiconductor epitaxial layer B. The material of substrate A includes but is not limited to sapphire, silicon, silicon carbide, gallium oxide, lithium aluminate, lithium niobate, germanium, aluminum nitride, zinc oxide, boron nitride, or lithium gallate; the doping type of the intentionally doped GaN layer can be p-type doping or n-type doping, and the intentionally doped GaN layer is used to conduct current.
[0047] S2, depositing a first etching mask layer C on the III-nitride semiconductor epitaxial layer B, such as Figure 2a shown.
[0048] Specifically, a dielectric film may be deposited on the III-nitride semiconductor epitaxial layer by a plasma enhanced chemical vapor deposition process as the first etching mask layer C. The material of the first etching mask layer C includes but is not limited to SiO2, SiN x , any one of TiO2.
[0049] S3, preparing a glue layer D having a periodic arrangement pattern on the first etching mask layer C, such as Figure 2b shown.
[0050] Specifically, the adhesive layer D includes ultraviolet photoresist, electron beam photoresist or nano-imprinting adhesive.
[0051] When the adhesive layer D is made of ultraviolet photoresist or electron beam photoresist, step S3 includes: coating photoresist on the first etching mask layer C, then using a photolithography machine to expose the pattern containing the nanoscale array, and developing it to obtain a photoresist layer D having a periodic arrangement pattern, wherein the portion of the periodic arrangement pattern has no photoresist, and the first etching mask layer C is exposed.
[0052] When the adhesive layer D is made of nanoimprint adhesive, step S3 includes: coating the nanoimprint adhesive on the first etching mask layer C, imprinting the nanoimprint adhesive to form a pattern including a nanoscale array, and then using a stripping process to thin the bottom of the patterned portion of the patterned nanoimprint adhesive until it is removed to expose the first etching mask layer, thereby forming a nanoimprint adhesive layer D having a periodically arranged pattern.
[0053] Specifically, the periodic arrangement pattern may be periodically arranged polygonal holes or circular holes, and the characteristic size thereof is nanometer scale.
[0054] S4, depositing a mask material on the glue layer D and in the periodic arrangement pattern, and peeling off the mask material on the surface of the glue layer D, forming a patterned second etching mask layer E on the first etching mask layer C, such as Figure 2c shown.
[0055] Specifically, a layer of dielectric film or metal film is evaporated and deposited on the surface of the sample (i.e., the glue layer D and the periodically arranged pattern) as a mask material, and a thin film stripping process is performed to strip the glue layer D and the mask material on the surface of the glue layer D, thereby forming a patterned second etching mask layer E on the first etching mask layer C.
[0056] Specifically, the ratio of the thickness / etching rate of the first etch mask layer C is smaller than the ratio of the thickness / etching rate of the second etch mask layer E, so that when the first etch mask layer C is etched, the surface of the unetched area is always covered by the second etch mask layer E. It can be understood that at the same thickness, the etching rate of the second etch mask layer E is smaller than the etching rate of the first etch mask layer C; at the same etching rate, the thickness of the first etch mask layer C is smaller than the thickness of the second etch mask layer E; however, the first etch mask layer C and the second etch mask layer E in this embodiment are not limited to the above situations, and the requirements of the ratio of thickness / etching rate can be met.
[0057] Specifically, the material of the second etching mask layer E includes a dielectric material or a metal material; the dielectric material includes Al2O3, and the metal material includes but is not limited to any one of Ni, Ti, and Cr.
[0058] Furthermore, the patterned second etching mask layer E is formed by a plurality of periodically arranged nanorods.
[0059] S5, dry-etching the first etching mask layer C until the surface of the III-nitride semiconductor epitaxial layer B in the area not covered by the second etching mask layer E is exposed, so that the pattern of the second etching mask layer E is transferred to the first etching mask layer C, and the patterned second etching mask layer E is removed to form a patterned first etching mask layer F, such as Figure 2d shown.
[0060] Specifically, the patterned first etching mask layer F is formed by a plurality of periodically arranged nanorods.
[0061] S6, dry etching the III-nitride semiconductor epitaxial layer B not covered by the patterned first etching mask layer F, so that the pattern of the patterned first etching mask layer F is transferred to the III-nitride semiconductor epitaxial layer B, and the patterned first etching mask layer F is removed to form a III-nitride semiconductor current spreading layer G and a patterned III-nitride semiconductor nanocolumn array template H, such as Figure 2e shown.
[0062] Specifically, when the III-nitride semiconductor epitaxial layer B includes a GaN nucleation layer, an unintentionally doped GaN layer, and an intentionally doped GaN layer stacked from bottom to top, the intentionally doped GaN layer not covered by the patterned first etching mask layer F is dry-etched, and the etching depth can be less than the thickness of the intentionally doped GaN layer, so that the pattern of the patterned first etching mask layer F is transferred to the intentionally doped GaN layer, and a periodically arranged nanoscale columnar structure is formed on the intentionally doped GaN layer. Then, the patterned first etching mask layer F is etched away to obtain a III-nitride semiconductor current spreading layer G and a patterned III-nitride semiconductor nanocolumn array template H. Among them, the patterned III-nitride semiconductor nanocolumn array template H is formed by a number of periodically arranged nanocolumns, and the bottom of the patterned III-nitride semiconductor nanocolumn array template H is a III-nitride semiconductor current spreading layer G, which includes a GaN nucleation layer, an unintentionally doped GaN layer and an unetched intentionally doped GaN layer stacked from bottom to top.
[0063] Specifically, in the group III nitride semiconductor nanocolumn array template H, the height of the nanocolumns is 100 nm to 5000 nm, the diameter of the nanocolumns is 50 nm to 1000 nm, and the distance between adjacent nanocolumns is 30 nm to 5000 nm.
[0064] It should be noted that in the III-nitride semiconductor nanocolumn array template H obtained in step S6, the sidewalls of the nanocolumns are inclined sidewalls with an inclination angle of about 75 to 85 degrees. The above-mentioned nanocolumn diameter refers to the diameter of the top of the nanocolumn, and the distance between adjacent nanocolumns is also the distance between the tops of adjacent nanocolumns.
[0065] Further, after obtaining the group III nitride semiconductor nanopillar array template H, the group III nitride semiconductor nanopillar array template H can be soaked in an alkaline solution to etch the nanopillars with inclined sidewalls into nanopillars with vertical sidewalls. Specifically, the alkaline solution can be a KOH solution, a NaOH solution, or an organic alkaline solution (e.g., a TMAH solution).
[0066] It should be noted that after obtaining the group III nitride semiconductor nanorod array template H, the step of soaking in an alkaline solution may not be performed.
[0067] S7, growing a first doping type III nitride semiconductor layer J, an active region K, and a second doping type III nitride semiconductor layer L on the III nitride semiconductor nanorod array template H in order from bottom to top to obtain a nanoscale visible light emitting diode, such as Figure 2f As shown, the active region K includes a quantum confinement layer, and the material of the quantum confinement layer includes an In-containing Group III nitride semiconductor.
[0068] Specifically, a first doping type III-nitride semiconductor layer J, an active region K, and a second doping type III-nitride semiconductor layer L are sequentially grown from bottom to top on a III-nitride semiconductor nanocolumn array template by MOCVD or molecular beam epitaxy to obtain a nanoscale visible light emitting diode. While growing the first doping type III-nitride semiconductor layer J, the shape of the nanocolumns in the III-nitride semiconductor nanocolumn array template H is changed to hexagonal columns I.
[0069] Specifically, the doping types of the first doping type III-nitride semiconductor layer J and the second doping type III-nitride semiconductor layer L are opposite, that is, the first doping type is n-type and the second doping type is p-type, or the first doping type is p-type and the second doping type is n-type.
[0070] Furthermore, the doping type of the intentionally doped GaN layer in the III-nitride semiconductor epitaxial layer B and the first doping type III-nitride semiconductor layer J may be the same or different. That is, when the first doping type is n-type, the intentionally doped GaN layer may be n-type doped or p-type doped; when the first doping type is p-type, the intentionally doped GaN layer may be n-type doped or p-type doped. Exemplarily, the intentionally doped GaN layer is an n-type doped GaN layer, the first doping type III-nitride semiconductor layer J is an n-type doped GaN layer, and the second doping type III-nitride semiconductor layer L is a p-type doped GaN layer.
[0071] Specifically, the Ga contents of the first doping type III-nitride semiconductor layer J and the second doping type III-nitride semiconductor layer L are both not less than 70%.
[0072] In a specific embodiment, the active region K includes a quantum confinement layer, a barrier layer and an electron blocking layer. Among them, a plurality of quantum confinement layers and a plurality of barrier layers are alternately stacked, and the quantum confinement layer is arranged between two adjacent barrier layers; the electron blocking layer is arranged on the upper surface of the top barrier layer, or the electron blocking layer is arranged on the lower surface of the bottom barrier layer.
[0073] Specifically, a plurality of barrier layers are distributed from bottom to top, and a quantum confinement layer is disposed between two adjacent barrier layers, forming a barrier layer, quantum confinement layer, barrier layer, ..., quantum confinement layer, barrier layer structure. The electron blocking layer can be disposed on the upper surface of the uppermost barrier layer, or on the lower surface of the lowermost barrier layer.
[0074] In another specific embodiment, the active region K includes a stress adjustment layer, a quantum confinement layer, a barrier layer and an electron blocking layer. The quantum confinement layer and the barrier layer are alternately stacked, and the quantum confinement layer is arranged between two adjacent barrier layers; the stress adjustment layer is arranged on the lower surface of the bottom barrier layer, and the electron blocking layer is arranged on the upper surface of the top barrier layer, or the electron blocking layer and the stress adjustment layer are stacked from top to bottom on the lower surface of the bottom barrier layer.
[0075] Specifically, a plurality of barrier layers are distributed from bottom to top, and a quantum confinement layer is arranged between two adjacent barrier layers, forming a barrier layer, a quantum confinement layer, a barrier layer, ..., a quantum confinement layer, a barrier layer structure. The electron blocking layer can be arranged on the upper surface of the uppermost barrier layer, in which case the stress adjustment layer is arranged on the lower surface of the bottom barrier layer. The electron blocking layer can also be arranged on the lower surface of the lowermost barrier layer, in which case the stress adjustment layer is arranged on the lower surface of the electron blocking layer.
[0076] Exemplarily, the quantum confinement layer can emit light with a wavelength of 380 to 780 nm under external excitation; the material of the barrier layer includes GaN; and the material of the electron blocking layer includes AlGaN.
[0077] It should be noted that the active region K includes the In-containing quantum confinement layer, and other layers can be arranged according to device requirements.
[0078] This embodiment also provides a nanoscale visible light emitting diode, which is prepared by the above preparation method.
[0079] like Figure 2f As shown, the nanoscale visible light emitting diode comprises a III-nitride semiconductor current spreading layer G, a patterned III-nitride semiconductor nanocolumn array template I, a first doping type III-nitride semiconductor layer J, an active region K, and a second doping type III-nitride semiconductor layer L. Among them, the nanocolumn array in the patterned III-nitride semiconductor nanocolumn array template I is arranged on the III-nitride semiconductor current spreading layer G and presents a periodic arrangement; each nanocolumn is provided with a first doping type III-nitride semiconductor layer J, an active region K, and a second doping type III-nitride semiconductor layer L stacked sequentially from bottom to top.
[0080] In a specific embodiment, the nanoscale visible light emitting diode further includes a substrate A, which is located on the lower surface of the III-nitride semiconductor current spreading layer G. It can be understood that the substrate A can be retained or peeled off according to device requirements.
[0081] In this embodiment, the first etching mask layer and the second etching mask layer are used to perform two dry etching processes to transfer the periodically arranged pattern to the III-nitride semiconductor epitaxial layer to form a patterned III-nitride semiconductor nanocolumn array template. The larger specific surface area of the nanocolumns allows the strong compressive strain of the active region grown on the nanocolumn array template to be partially relaxed, which can reduce the energy required for In incorporation and effectively increase the incorporation of In in the In-containing quantum confinement layer, thereby achieving long-wavelength emission; at the same time, since the strong compressive strain of the active region is partially relaxed, the piezoelectric polarization field in the In-containing quantum confinement layer is weakened, thereby effectively reducing the influence of the quantum confined Stark effect on the energy band, improving the radiation recombination efficiency, and increasing the luminous intensity of the light-emitting diode;
[0082] The nanoscale visible light emitting diode of this embodiment has a three-dimensional vertical structure, and the sidewalls can effectively extract light, which is beneficial to improving the light extraction efficiency, thereby improving the external quantum efficiency of the light emitting diode.
[0083] The active region of the nanoscale visible light LED of this embodiment is not dry-etched, thereby avoiding etching damage on the sidewalls of the LED structure.
[0084] Embodiment 2
[0085] Based on the first embodiment, this embodiment further specifically describes the preparation method of nanoscale visible light emitting diodes and their beneficial effects.
[0086] See also Figure 2a-2f The method for preparing the nanoscale visible light emitting diode comprises the following steps:
[0087] S1. Growing a III-nitride semiconductor epitaxial layer B on a substrate A, such as Figure 2a shown.
[0088] Specifically, a sapphire substrate A with a thickness of 650 μm was prepared, and the sapphire substrate A was placed in a reaction chamber of a metal organic vapor phase epitaxy system, and the sapphire substrate A was heated to raise the temperature to 1100° C., and the sapphire substrate A was subjected to high temperature treatment for 20 minutes in a hydrogen atmosphere, and the temperature was lowered to 515° C., and ammonia was introduced into the reaction chamber for 3 minutes, and then hydrogen and TMGa were introduced to epitaxially grow a 20 nm GaN nucleation layer, and the temperature was raised to 1050° C., and hydrogen, TMGa and ammonia were introduced to epitaxially grow a 1 μm thick non-intentionally doped GaN layer and a 2 μm thick n-type doped GaN layer, and SiH4 was introduced simultaneously when growing the n-type doped GaN layer, and the doping concentration was 5×10 18 cm -3 , completing the preparation of planar n-type doped GaN template. Figure 1In the figure, A is a sapphire substrate; B is a III-nitride semiconductor epitaxial layer, including a nucleation layer, an unintentionally doped GaN layer and an n-type doped GaN layer.
[0089] S2. Depositing a first etching mask layer C on the III-nitride semiconductor epitaxial layer B.
[0090] Specifically, a 500 nm thick SiO2 layer is deposited on the surface of the n-type doped GaN layer by a plasma enhanced chemical vapor deposition process as the first etching mask layer C, and the obtained structure is as follows: Figure 2a shown.
[0091] S3, preparing a glue layer D having a periodically arranged pattern on the first etching mask layer C.
[0092] Specifically, a photoresist with a thickness of 600 nm is uniformly spin-coated on the surface of the SiO2 layer of the substrate obtained in step S2, and a pattern containing a nanoscale circular array is exposed using a stepper lithography machine, and then developed to obtain a photoresist layer D containing a periodic array of nanoscale photoresist holes, such as Figure 2b As shown, the period of the array (the distance between the centers of adjacent holes) is 800 nm, the diameter of the holes is 400 nm, and the distance between the holes is 400 nm.
[0093] S4 , depositing a mask material on the glue layer D and in the periodically arranged pattern, and stripping the mask material on the surface of the glue layer D to form a patterned second etching mask layer E on the first etching mask layer C.
[0094] Specifically, a patterned photoresist layer is placed in a chamber of an electron beam evaporation deposition device, nickel with a thickness of 100 nm is deposited, then taken out and placed in acetone, heated in a water bath at 50° C. for 60 minutes to dissolve the photoresist and peel off the nickel on the surface of the photoresist, then placed in isopropanol and water for ultrasonic cleaning for 10 minutes in turn, taken out and dried with nitrogen, and a patterned nickel layer E is obtained on the surface of the SiO2 layer as a patterned second etching mask layer E, and the patterned second etching mask layer E is formed by a plurality of periodically arranged nanopillars, such as Figure 2c shown.
[0095] S5. Dry-etch the first etch mask layer C until the surface of the III-nitride semiconductor epitaxial layer B in the area not covered by the second etch mask layer E is exposed, so that the pattern of the second etch mask layer E is transferred to the first etch mask layer C, and the patterned second etch mask layer E is removed to form a patterned first etch mask layer F.
[0096] Specifically, a substrate having a patterned nickel layer E on the surface is placed in a chamber of an inductively coupled plasma etcher, and the SiO2 layer is etched by an inductively coupled plasma etching process in a carbon tetrafluoride and argon atmosphere using the patterned nickel layer E as a mask, and the SiO2 not covered by nickel is etched, and a SiO2 column array is formed in the area covered by nickel, and then a nickel etching solution is placed until the nickel is removed, and a SiO2 column array F is obtained on a planar n-type doped GaN template as a patterned first etching mask layer F, and the SiO2 column array F is formed by a plurality of periodically arranged nanocolumns, such as Figure 2d shown.
[0097] S6. Dry-etching the III-nitride semiconductor epitaxial layer B not covered by the patterned first etching mask layer F, so that the pattern of the patterned first etching mask layer F is transferred to the III-nitride semiconductor epitaxial layer B, and removing the patterned first etching mask layer F to form a III-nitride semiconductor current spreading layer G and a patterned III-nitride semiconductor nanocolumn array template H.
[0098] Specifically, a planar n-type doped GaN template having a patterned SiO2 column array F on its surface is placed in a chamber of an inductively coupled plasma etcher, and the n-type GaN template is etched by 750 nm using an inductively coupled plasma etching process in an atmosphere of chlorine and argon, that is, a portion of the thickness of the n-type doped GaN layer is etched in a vertical direction, and the n-type doped GaN not covered by the SiO2 column array is etched, and a GaN column array is formed in the area covered by the SiO2 column array, and then a buffered oxide etching solution is placed until the SiO2 column array mask is etched, thereby obtaining an n-type doped GaN nanocolumn array template H, as shown in FIG. Figure 2e As shown, the side wall of the column has a certain inclination angle, and below is the III-nitride semiconductor current spreading layer G, which includes the remaining unetched n-type doped GaN layer, the unintentionally doped GaN layer and the nucleation layer from top to bottom.
[0099] S7, soaking the group III nitride semiconductor nanorod array template H in an alkaline solution to etch the nanorods with inclined side walls into nanorods with vertical side walls.
[0100] Specifically, the obtained n-type doped GaN nanorod array template was placed in a 5% TMAH solution at 45° C. and etched for 30 minutes, so that the side wall changed from inclined to vertical.
[0101] S8, growing a first doping type III nitride semiconductor layer J, an active region K, and a second doping type III nitride semiconductor layer L on the III nitride semiconductor nanorod array template H in sequence from bottom to top to obtain a nanoscale visible light emitting diode, such as Figure 2f shown.
[0102] Specifically, the n-type doped GaN nanocolumn array template is placed in a reaction chamber of a metal organic vapor deposition system to epitaxially grow a light emitting diode structure, which specifically includes the following steps:
[0103] S81, the temperature of the reaction chamber is raised to 1020°C, TMGa, SiH4, ammonia, nitrogen and hydrogen are introduced, and a 100nm thick n-type doped GaN layer J is grown on the columnar structure, and the concentration of n-type doping is 5×10 18 cm -3 , and at the same time, the shape of the GaN nanocolumn changes to a hexagonal column I.
[0104] S82, start growing the active region K, including the stress adjustment layer, the quantum confinement layer, the barrier layer and the electron blocking layer.
[0105] Specifically, the temperature is first lowered to 900°C, and the gases are switched to TEGa, TMIn, SiH4, ammonia, nitrogen and hydrogen to grow an InGaN / GaN superlattice structure with a thickness of 80nm to form a stress adjustment layer; the InGaN layer of the stress adjustment layer has an In content of not less than 5%. Then the SiH4 is stopped, and 10 cycles of InGaN quantum confinement layers and GaN barrier layers are grown alternately; wherein the number of layers of the InGaN quantum confinement layer is 10, the growth temperature is 640°C, and the thickness is 3nm; the number of layers of the GaN barrier layer is 11, the growth temperature is 800°C, and the thickness is 9nm. Then the gases are switched to TMGa, TMAl, ammonia and hydrogen to grow a 20nm thick AlGaN electron blocking layer with an Al content of not less than 5%.
[0106] S83, grow a p-type doped GaN layer L, switch the gas to TEGa, bismuth magnesium, ammonia, nitrogen and hydrogen, grow a thickness of 180nm, and the p-type doping concentration is 1×10 19 cm -3 , complete the epitaxial growth of light-emitting diode devices, such as Figure 2f shown.
[0107] The active area of the light-emitting diode grown by the preparation method of this embodiment is not dry-etched, which avoids etching damage on the sidewalls. The nanometer-scale columnar structure can also partially relax the compressive stress and promote the incorporation of In. Figure 3 , Figure 3 This is a comparison chart of the normalized luminescence spectrum of the nanoscale light-emitting diode prepared by the preparation method of the embodiment of the present invention and the normalized luminescence spectrum of the light-emitting diode obtained by using a traditional plane template, wherein the solid line is the nanoscale light-emitting diode prepared by the preparation method of the embodiment of the present invention, and the dotted line is the light-emitting diode obtained by using a traditional plane template. Figure 3It can be seen that the peak wavelength of the spectrum of the solid line is longer than that of the dotted line, indicating that the InGaN quantum confinement layer in its active region has a higher In content.
[0108] In this embodiment, two dielectric or metal films with different etching rates are sequentially deposited on a planar GaN, and after two dry etchings, a stress relaxation patterned GaN template is formed, and then an n-type doped GaN layer, an active region and a p-type doped GaN layer are sequentially grown on the stress relaxation patterned GaN template to obtain a nanoscale light-emitting diode. The strong compressive strain of the n-type doped GaN and the active region grown on the stress relaxation patterned GaN template is partially relaxed, and the piezoelectric polarization field existing in the In-containing quantum confinement layer is weakened, thereby effectively reducing the influence of the quantum confined Stark effect on the energy band, improving the radiative recombination efficiency, and increasing the luminous intensity of the light-emitting diode. At the same time, the energy required for In incorporation is reduced, and the incorporation of In in the In-containing quantum confinement layer is effectively increased, thereby increasing the wavelength of the light.
[0109] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a nanoscale visible light emitting diode, It is characterized in that Includes steps: S1, growing a III-nitride semiconductor epitaxial layer on a substrate; S2, depositing a first etching mask layer on the III-nitride semiconductor epitaxial layer; S3, preparing a glue layer having a periodically arranged pattern on the first etching mask layer; S4, depositing a mask material on the glue layer and in the periodic arrangement pattern, and stripping the mask material on the surface of the glue layer to form a patterned second etching mask layer on the first etching mask layer; S5, dry-etching the first etch mask layer until the surface of the III-nitride semiconductor epitaxial layer in the area not covered by the patterned second etch mask layer is exposed, so that the pattern of the second etch mask layer is transferred to the first etch mask layer, and removing the patterned second etch mask layer to form a patterned first etch mask layer; S6, dry-etching the III-nitride semiconductor epitaxial layer not covered by the patterned first etching mask layer, so that the pattern of the patterned first etching mask layer is transferred to the III-nitride semiconductor epitaxial layer, and removing the patterned first etching mask layer to form a III-nitride semiconductor current spreading layer and a patterned III-nitride semiconductor nanocolumn array template; S7. Growing a first doping type III nitride semiconductor layer, an active region, and a second doping type III nitride semiconductor layer on the III nitride semiconductor nanocolumn array template from bottom to top in sequence to obtain a nanoscale visible light emitting diode, wherein the active region includes a quantum confinement layer, and the material of the quantum confinement layer includes an In-containing III nitride semiconductor.
2. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that Step S1 includes: Growing a GaN nucleation layer, an unintentionally doped GaN layer, and an intentionally doped GaN layer on the substrate in sequence to form the III-nitride semiconductor epitaxial layer; The doping type of the intentionally doped GaN layer includes n-type doping or p-type doping.
3. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that A ratio of the thickness of the first etch mask layer to the etching rate is smaller than a ratio of the thickness of the second etch mask layer to the etching rate.
4. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that The adhesive layer includes ultraviolet photoresist, electron beam photoresist or nano-imprinting adhesive.
5. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that The height of the nanocolumns in the III-nitride semiconductor nanocolumn array template is 100nm to 5000nm, the diameter of the nanocolumns is 50nm to 1000nm, and the distance between adjacent nanocolumns is 30nm to 5000nm.
6. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that Before step S7, the method further includes: The group III nitride semiconductor nano-column array template is immersed in an alkaline solution to etch the nano-columns with inclined side walls into nano-columns with vertical side walls.
7. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that The first doping type includes n-type, and the second doping type includes p-type, or the first doping type includes p-type, and the second doping type includes n-type; The Ga contents of the first doping type III-nitride semiconductor layer and the second doping type III-nitride semiconductor layer are both not less than 70%.
8. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that The active region includes a plurality of quantum confinement layers, a plurality of potential barrier layers and an electron blocking layer, wherein: The plurality of quantum confinement layers and the plurality of barrier layers are alternately stacked, and the quantum confinement layer is arranged between two adjacent barrier layers; The electron blocking layer is arranged on the upper surface of the top barrier layer, or the electron blocking layer is arranged on the lower surface of the bottom barrier layer; The quantum confinement layer can emit visible light with a wavelength of 380 to 780 nm under external excitation.
9. The method for preparing a nanoscale visible light emitting diode according to claim 1, It is characterized in that The active region includes a stress adjustment layer, a quantum confinement layer, a barrier layer and an electron blocking layer, wherein: The quantum confinement layers and the barrier layers are alternately stacked, and the quantum confinement layer is arranged between two adjacent barrier layers; The stress adjustment layer is arranged on the lower surface of the bottom barrier layer, and the electron blocking layer is arranged on the upper surface of the top barrier layer, or the electron blocking layer and the stress adjustment layer are stacked on the lower surface of the bottom barrier layer from top to bottom; The quantum confinement layer can emit visible light with a wavelength of 380 to 780 nm under external excitation.
10. A nanoscale visible light emitting diode, It is characterized in that Prepared by the preparation method according to any one of claims 1 to 9, comprising: a group III nitride semiconductor current spreading layer, a patterned group III nitride semiconductor nanocolumn array template, a first doping type group III nitride semiconductor layer, an active region and a second doping type group III nitride semiconductor layer, wherein: The nanocolumn array in the patterned III-nitride semiconductor nanocolumn array template is arranged on the III-nitride semiconductor current spreading layer and presents a periodic arrangement; A first doping type III-nitride semiconductor layer, an active region, and a second doping type III-nitride semiconductor layer are sequentially stacked from bottom to top on each nanocolumn.
Citation Information
Patent Citations
Method for growing group III nitride nanometer material
CN101898751A
Nanoimprinting method capable of improving depth-to-width ratio of graph and product thereof
CN102910579A
Nano-column ultraviolet LED and preparation method and application thereof
CN108493309A
Group III nitride substrate preparation method and semiconductor device
CN112802930A
Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode
CN116404079A
Cited By
LED chip structure and preparation method thereof
CN120051067A