Low-residual-alkali high-nickel positive electrode material as well as preparation method and application thereof

By using the coating technology of AlCl3 layer and porous γ-Al2O3 particles on the high-nickel positive electrode material, the problems of high residual alkali and coating and shedding in the high-nickel positive electrode material are solved, and low residual alkali, high specific capacity and good cycles are achieved The performance effect simplifies the preparation process and improves production efficiency.

CN119050307AActive Publication Date: 2024-11-29四川新能源汽车创新中心有限公司

Patent Information

Application Number
CN202411182988.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

When the nickel content of the existing high-nickel cathode materials increases, the high residual alkali leads to uneven preparation process, safety hazards and poor circulation performance. In addition, the traditional coating method has problems of shedding, making it difficult to reduce residual alkali quickly, efficiently and controllably.

Method used

The AlCl3 layer and porous γ-Al2O3 particles embedded in the AlCl3 layer were coated, and the surface was washed and coated simultaneously through the organic-inorganic interface. The coating was fixed by low-temperature sintering, reducing residual alkali and improving the coating strength.

Benefits of technology

It achieves low residual alkali, high specific capacity and good cycle performance, simplifies the preparation process, reduces experimental complexity and uncontrollable factors, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050307A_ABST
    Figure CN119050307A_ABST
Patent Text Reader

Abstract

The invention discloses a low-residual-alkali high-nickel positive electrode material as well as a preparation method and application thereof. The low-residual alkali high-nickel positive electrode material provided by the invention comprises a substrate and a coating layer on the surface of the substrate, the substrate is a high-nickel positive electrode material, the coating layer comprises an AlCl3 layer and porous gamma-Al2O3 particles embedded in the AlCl3 layer, and at least part of the porous gamma-Al2O3 particles are in contact with the high-nickel positive electrode material. Through an organic-inorganic interface formed in a dispersion system, the step of washing the high-nickel positive electrode material to reduce residual alkali and the step of coating the surface of the high-nickel positive electrode material are respectively carried out in an upper-layer water phase and a lower-layer organic phase, so that washing and surface coating are synchronously carried out, and then low-temperature sintering is carried out; the porous gamma-Al2O3 particles are fixed on the surface of the high-nickel positive electrode material by using the AlCl3 film, so that the porous gamma-Al2O3 particles are not easy to fall off. The low-residual alkali high-nickel positive electrode material prepared by the method has the advantages of low residual alkali value, high specific capacity and good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a low-residual-alkali high-nickel positive electrode material and a preparation method and application thereof. Background Art

[0002] With the rapid development of new energy, the demand for energy density is getting higher and higher, and high-nickel cathode materials are currently the best choice. However, as the nickel content increases, the residual alkali in high-nickel cathode materials becomes higher and higher. High residual alkali not only affects the homogenization and coating of the preparation process, but also produces gas during the cycle, causing flatulence and safety accidents, and the cycle performance also deteriorates.

[0003] At present, the main ways to reduce residual alkali include adjusting the raw material ratio and the first calcination process, water washing and coating, and dry coating. Among them, water washing followed by coating is the most effective way to reduce residual alkali. However, there are many factors that affect water washing, including water-to-material ratio, water washing time, and stirring intensity. The process for each material is different, the experimental intensity is high, and the experimental cycle is long. At the same time, the coating is mostly done by dot-shaped or surface coating of inorganic materials. After coating, it is easy to fall off from the high-nickel positive electrode material as the volume of the high-nickel positive electrode material shrinks and expands during charging.

[0004] How to reduce residual alkali quickly, efficiently and controllably, and achieve more effective coating has become an urgent problem to be solved. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a low-residual-alkali high-nickel positive electrode material and a preparation method and application thereof.

[0006] The present invention solves the technical problem by adopting the following technical solutions.

[0007] The present invention provides a low residual alkali high nickel positive electrode material, comprising a substrate and a coating layer on the surface of the substrate, wherein the substrate is a high nickel positive electrode material, the coating layer comprises an AlCl3 layer and porous γ-Al2O3 particles embedded in the AlCl3 layer, and at least part of the porous γ-Al2O3 particles are in contact with the high nickel positive electrode material.

[0008] The present invention also provides a method for preparing the above-mentioned low residual alkali high nickel positive electrode material, comprising: adding water to an organic solvent containing the high nickel positive electrode material to obtain a dispersed system of an upper aqueous phase and a lower organic phase; stirring the high nickel positive electrode material to move upward into the upper aqueous phase, and washing with water to remove the residual alkali on the surface of the high nickel positive electrode material; depositing and adsorbing Al(OH)3 on the surface of the high nickel positive electrode material, and then coating the high nickel positive electrode material with AlCl3; and finally performing low temperature sintering to obtain the low residual alkali high nickel positive electrode material.

[0009] The present invention also provides a lithium battery, wherein the positive electrode of the lithium battery comprises the above-mentioned low residual alkali high nickel positive electrode material.

[0010] The present invention has the following beneficial effects:

[0011] The present invention provides a low residual alkali high nickel positive electrode material and a preparation method and application thereof. The low residual alkali high nickel positive electrode material provided by the present invention comprises a substrate and a coating layer on the surface of the substrate, wherein the substrate is a high nickel positive electrode material, and the coating layer comprises an AlCl3 layer and porous γ-Al2O3 particles embedded in the AlCl3 layer, and at least part of the porous γ-Al2O3 particles are in contact with the high nickel positive electrode material. In the present invention, the step of washing the high nickel positive electrode material to reduce the residual alkali and the step of coating the surface of the high nickel positive electrode material are respectively carried out in the upper aqueous phase and the lower organic phase through the organic-inorganic interface formed in the dispersion system, so that the washing and the surface coating are carried out simultaneously, and then low temperature sintering is carried out, and the porous γ-Al2O3 particles are fixed on the surface of the high nickel positive electrode material by using an AlCl3 film, and the fixed coating is not easy to fall off on the surface of the high nickel positive electrode material. The low residual alkali high nickel positive electrode material prepared by the present invention has the advantages of low residual alkali value, high specific capacity and good cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0013] Figure 1 This is a schematic diagram of the structure of a low residual alkali high nickel positive electrode material prepared in an embodiment of the present invention;

[0014] Figure 2 Schematic diagram of the experimental process for preparing a low residual alkali high nickel positive electrode material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0016] High nickel cathode materials have rapidly become one of the preferred high nickel cathode materials for high specific energy batteries due to their advantages such as high voltage platform, high energy density and high tap density. However, with the increase of nickel content, the structural stability of high nickel cathode materials deteriorates, resulting in low cycle stability. Improving the structural stability of high nickel cathode materials by surface coating is an effective solution. For example, materials such as AIF3, A1203 and Li3PO4 are common surface coatings, but the coating with the above materials is mostly surface point or surface coating. The coating is simply dispersed on the surface of the high nickel cathode material by physical adsorption. The binding force between the two is not strong, and there is a gap between the two. The expansion and contraction of the high nickel cathode material can easily cause the coating to fall off.

[0017] In order to achieve more effective and stable coating, an embodiment of the present invention provides a method for preparing a low-residual-alkali high-nickel positive electrode material, which comprises: firstly setting a dispersion system of an upper aqueous phase and a lower organic phase containing a high-nickel positive electrode material, and then, through the construction of an organic-inorganic interface, washing to remove residual alkali and surface coating are respectively performed above and below the interface, specifically: stirring is used to flip the high-nickel positive electrode material upward, water removes residual alkali on the surface of the high-nickel positive electrode material, an organic solvent reduces the contact between water and the high-nickel positive electrode material, and protects the high-nickel positive electrode material from being further damaged by water, thereby achieving the removal of residual alkali from the high-nickel positive electrode material above the organic-inorganic interface, and monitoring the effect of the high-nickel positive electrode material in removing residual alkali by online detection of the pH value of the aqueous solution, so as to prepare a low-residual-alkali and high-nickel positive electrode material in one step. The high-nickel positive electrode material whose structure is not damaged is moved downward under the action of gravity to separate the high-nickel positive electrode material from water; then, the hydrolysis characteristics of aluminate are used to hydrolyze in the upper aqueous solution to generate Al(OH)3 precipitate, and the Al(OH)3 precipitate settles into the lower organic solvent and is adsorbed and coated on the surface of the high-nickel positive electrode material, and then AlCl3 solution is added to the organic solvent to make it also coated on the surface of the high-nickel positive electrode material to obtain a coated precursor; finally, low-temperature calcination is performed, and Al(OH)3 is transformed into porous γ-Al2O3 particles at low temperature. At the same time, the porous γ-Al2O3 particles are "shaped" and coated with AlCl3 with a low melting point, so that the coating is fixed on the surface of the high-nickel positive electrode material and is not easy to fall off, thereby increasing the coating contact effect and the coating strength.

[0018] The following is a detailed description of a low residual alkali high nickel positive electrode material provided by the present invention and its preparation method and application:

[0019] In the first aspect, an embodiment of the present invention provides a low residual alkali high nickel positive electrode material, including a substrate and a coating layer on the surface of the substrate, wherein the substrate is a high nickel positive electrode material, the coating layer includes an AlCl3 layer and porous γ-Al2O3 particles embedded in the AlCl3 layer, and at least part of the porous γ-Al2O3 particles are in contact with the high nickel positive electrode material.

[0020] See also Figure 1 In the low residual alkali high nickel positive electrode material provided by an embodiment of the present invention, the distribution of porous γ-Al2O3 particles embedded in the AlCl3 layer may be varied, such as some porous γ-Al2O3 particles penetrate the AlCl3 layer and are connected to the high nickel positive electrode material, some porous γ-Al2O3 particles are connected to the high nickel positive electrode material but do not penetrate the AlCl3 layer, some porous γ-Al2O3 particles are completely embedded in the AlCl3 layer, and some porous γ-Al2O3 particles are only partially embedded in the AlCl3 layer and are not in contact with the high nickel positive electrode material.

[0021] It can be seen that the low residual alkali high nickel positive electrode material provided by the embodiment of the present invention utilizes the "shaping" coating effect of AlCl3 to achieve the solidification of the porous γ-Al2O3 coating. It can be understood that the "shaping" coating mentioned here means that AlCl3 is coated on the surface of the high nickel positive electrode material in the form of a film, which can be formed according to the shape of the high nickel positive electrode material and is not easy to fall off. At the same time, AlCl3 fixes the porous γ-Al2O3 particles on the surface of the high nickel positive electrode material in the form of a film, so that the porous γ-Al2O3 particles are not easy to fall off, increase the coating contact effect, and increase the coating strength. At the same time, the porous γ-Al2O3 particles and AlCl3 film coated on the surface of the high nickel positive electrode material play the role of isolating the electrolyte and the high nickel positive electrode material. The porous and thin film design can also provide channels for lithium ions without reducing the capacity and rate.

[0022] In an optional embodiment, the chemical formula of the high nickel positive electrode material is LiNi x M 1-x O2, wherein 0.6≤x≤1.0, and M is selected from at least one of Co, Mn, and Al.

[0023] In an optional embodiment, the composition of the low residual alkali high nickel positive electrode material includes: LiNi x Mn y O2, LiNi x Co y O2, LiNi x Co y Mn z O2, LiNi x Co y Al z O2, LiNi x Co y Mn z Al w O2, etc.

[0024] In an optional embodiment, the thickness of the surface coating layer of the low residual alkali and high nickel positive electrode material is 0.5 nm-50 nm.

[0025] In the second aspect, an embodiment of the present invention also provides a method for preparing the above-mentioned low residual alkali high-nickel positive electrode material, comprising: adding water to an organic solvent containing a high-nickel positive electrode material to obtain a dispersed system of an upper aqueous phase and a lower organic phase; stirring the high-nickel positive electrode material to move upward into the upper aqueous phase, and washing with water to remove the residual alkali on the surface of the high-nickel positive electrode material; depositing and adsorbing Al(OH)3 on the surface of the high-nickel positive electrode material, and then coating the high-nickel positive electrode material with AlCl3; and finally performing low-temperature sintering to obtain a low residual alkali high-nickel positive electrode material.

[0026] See also Figure 2 The method for preparing the low residual alkali high nickel cathode material provided in the embodiment of the present invention can make the step of washing the high nickel cathode material to reduce the residual alkali and the step of surface coating the high nickel cathode material respectively carried out in the upper aqueous phase and the lower organic phase through the organic-inorganic interface formed in the dispersed system, so as to achieve the synchronization of washing and surface coating, and then carry out low temperature sintering to solidify the coating and increase the coating contact effect. Specifically:

[0027] Water is added to an organic solvent containing a high-nickel cathode material to obtain a dispersion system of an upper aqueous phase and a lower organic phase. The high-nickel cathode material is moved upward into the upper aqueous phase by stirring, and the residual alkali is washed with water. At the same time, the organic solvent is used to isolate water from further reaction with the high-nickel cathode material to protect the structure of the high-nickel cathode material from being destroyed. The residual alkali can be effectively reduced while protecting the structure of the high-nickel cathode material from being destroyed. The complexity of the traditional water washing process, which repeatedly adjusts the water-to-material ratio, water washing time, stirring intensity, and water temperature through orthogonal experiments, is reduced. At the same time, the uncontrollability of the high-nickel cathode material contacting with water during the process of adding, discharging, filtering, and drying is also eliminated, which greatly reduces uncontrollable factors and reduces the intensity of the experiment.

[0028] After washing the high-nickel cathode material in the upper aqueous phase to remove the residual alkali to obtain a high-nickel cathode material with qualified residual alkali, add aluminate to the mixed solution, use the water and pH value of the supernatant after washing to hydrolyze the aluminate to produce Al(OH)3 precipitate, and the Al(OH)3 precipitate produced at the same time settles to the lower organic phase and adsorbs on the surface of the high-nickel cathode material, then add AlCl3 solution to the lower organic solvent, and use AlCl3 to coat the high-nickel cathode material. Then, low-temperature sintering is performed, which can transform Al(OH)3 into solid porous γ-Al2O3 particles, and AlCl3 into liquid AlCl3. In this process, the porous γ-Al2O3 particles are embedded in AlCl3. After the temperature is cooled, AlCl3 solidifies to form an AlCl3 layer, which then contacts the high-nickel cathode material, and see again. Figure 1 , porous γ-Al2O3 particles of different morphologies and particle sizes are embedded in the AlCl3 layer, which increases the coating contact effect and the coating strength.

[0029] The above-mentioned method for preparing low residual alkali high nickel positive electrode material adopts low melting point AlCl3 to coat porous γ-Al2O3 particles so as to contact and coat with high nickel positive electrode material in a better form, and at the same time, it can prevent the volume expansion of high nickel positive electrode material during charging and discharging, causing porous γ-Al2O3 to fall off and lose the coating effect. At the same time, the porous γ-Al2O3 particles and AlCl3 film coated on the surface of high nickel positive electrode material play the role of isolating electrolyte and high nickel positive electrode material, and the porous and film structure can also provide channels for lithium ions without reducing capacity and rate. It can be seen that the scheme provided by the embodiment of the present invention, through the constructed organic-inorganic interface, efficiently and quickly reduces the residual alkali content of high nickel positive electrode material and realizes the surface coating of high nickel positive electrode material. The preparation method provided by the embodiment of the present invention has a simple process, reduces a large number of positive electrode experiments, improves experimental efficiency, and the prepared low residual alkali high nickel positive electrode material has the advantages of low residual alkali value, high specific capacity and good cycle performance.

[0030] In an optional embodiment, the following steps are included:

[0031] The high-nickel cathode material is mixed with an organic solvent, stirred at a low speed, and then water is added to obtain a dispersion system of an upper aqueous phase and a lower organic phase;

[0032] The stirring speed is increased to make the high-nickel positive electrode material in the dispersed system contact with the upper aqueous phase to wash away the residual alkali on the surface of the high-nickel positive electrode material, and then the stirring speed is reduced to make the high-nickel positive electrode material sink to the lower organic phase to obtain a mixed solution with qualified residual alkali on the surface of the high-nickel positive electrode material;

[0033] Al(OH)3 is deposited and adsorbed on the surface of the high-nickel cathode material, and then AlCl3 solution is added to the lower organic phase, and the solid is collected by solid-liquid separation to obtain a coating precursor;

[0034] The coated precursor is sintered at low temperature to obtain a low residual alkali and high nickel positive electrode material.

[0035] In an optional embodiment, the preparation of the dispersion system includes: mixing the high-nickel positive electrode material with an organic solvent, starting low-speed stirring, controlling the high-nickel positive electrode material to have no precipitation, and then adding water to obtain a dispersion system of an upper aqueous phase and a lower organic phase;

[0036] Preferably, the organic solvent includes one or more of chloroform, carbon tetrachloride, ethylene dichloride, dibromomethane, bromoform, chlorobenzene, and carbon disulfide;

[0037] Preferably, the solid content in the dispersed system is 10%-70%;

[0038] Preferably, the stirring speed of the low-speed stirring is 0-150 rpm.

[0039] In an optional embodiment, the preparation of the mixed solution includes: increasing the stirring speed of the dispersion system, under high-speed stirring conditions, allowing the high-nickel positive electrode material to move upward and contact with water to wash away residual alkali, and an online pH value monitoring system to monitor the pH change in the water in real time, and when the pH reaches the target value, reducing the stirring speed to allow the high-nickel positive electrode material to sink and separate from the water;

[0040] Preferably, the stirring speed of high-speed stirring is 200-500 rpm, and the stirring speed of low-speed stirring is 0-150 rpm;

[0041] Preferably, the ratio of water to high nickel positive electrode material is controlled to be 0.5 to 30;

[0042] Preferably, the formula: "J 水洗后高镍正极材料残碱 =J 高镍正极材料初始残碱 -J 水溶剂碱 ” Calculate and determine the residual alkali content of high nickel positive electrode material in the solution, where: J 水溶剂碱 Detection using an online pH monitoring system;

[0043] Preferably, sampling is performed to detect the residual alkali content on the surface of the high-nickel positive electrode material. If the residual alkali value of the high-nickel positive electrode material is unqualified, stirring and monitoring are continued until the residual alkali value of the high-nickel positive electrode material is qualified.

[0044] The method for preparing the low residual alkali high nickel positive electrode material provided in the embodiment of the present invention utilizes online pH detection to monitor the pH value of the aqueous solution in real time, can monitor the water washing effect in real time, and can terminate the residual alkali washing reaction at any time by utilizing the organic-inorganic interface.

[0045] In an optional embodiment, the preparation of the coating precursor includes: adding aluminate to the mixed solution, using the Al(OH)3 produced by the hydrolysis of the aluminate to precipitate and adsorb to the surface of the high-nickel positive electrode material, after the Al(OH)3 precipitation is completed, extracting the supernatant, adding AlCl3 solution, and collecting the solid by solid-liquid separation to obtain the coating precursor;

[0046] Preferably, the metaaluminate includes one or more of NaAlO2 and KAlO2;

[0047] Preferably, the molar ratio of Al in the metaaluminate to the high-nickel positive electrode material is controlled to be 0.005%-2%;

[0048] Preferably, the molar ratio of AlCl3 to high-nickel positive electrode material in the AlCl3 solution is controlled to be 0.005%-2%;

[0049] Preferably, after the Al(OH)3 precipitation is completed, the supernatant is extracted, AlCl3 solution is added, and after mixing for 1 hour, the solid is collected by solid-liquid separation to obtain a coating precursor.

[0050] The preparation method of the above-mentioned low residual alkali high nickel positive electrode material provided by an embodiment of the present invention is to construct an organic-inorganic interface, add aluminate after completing water washing in the aqueous phase, and use the supernatant water and pH value after water washing to hydrolyze the aluminate to produce Al(OH)3. The addition rate of aluminate is controlled so that Al(OH)3 can be precipitated slowly and evenly and adsorbed onto the surface of the high nickel positive electrode material in the lower organic solvent. Thereafter, AlCl3 is added to the organic solvent and coated on the high nickel positive electrode material to obtain a coated precursor.

[0051] In an optional embodiment, the preparation of the low residual alkali high nickel positive electrode material comprises: sintering the coated precursor at 150° C.-300° C. for 2 h-10 h to obtain a crude product;

[0052] Preferably, sintering is carried out in an oxygen atmosphere, and the oxygen concentration is ≥ 99%;

[0053] Preferably, the method further comprises: cooling the crude product to below 80° C., taking it out, grinding and screening it, and obtaining a finished product of a low-residual-alkali and high-nickel positive electrode material;

[0054] Preferably, the heating rate and the cooling rate are both controlled to be 3°C / min.

[0055] The method for preparing the above-mentioned low residual alkali high nickel positive electrode material provided by the embodiment of the present invention is to sinter the coated precursor at low temperature after preparing the coated precursor. The low temperature sintering can transform the Al(OH)3 adsorbed on the surface of the high nickel positive electrode material into porous γ-Al2O3 particles, and at the same time, the low melting point AlCl3 on the surface of the high nickel positive electrode material plastically coats the porous γ-Al2O3 particles. Specifically:

[0056] The coated precursor is sintered at low temperature. During the low temperature sintering process, Al(OH)3 will be transformed into active porous γ-Al2O3 under the action of low temperature sintering. At the same time, AlCl3 on the surface of the high nickel positive electrode material is liquid at a temperature of 150℃-300℃, the porous γ-Al2O3 is solid, and AlCl3 is liquid. One solid and one liquid can be coated on the high nickel positive electrode material with better plasticity. That is, at a temperature higher than the melting point of AlCl3 (the melting point of AlCl3 is 194°C), AlCl3 is coated on the surface of the high-nickel positive electrode material in the form of a "film", and the porous γ-Al2O3 particles are embedded in the AlCl3. After the temperature is cooled, AlCl3 solidifies to form an AlCl3 layer, which better solidifies the porous γ-Al2O3 particles and the high-nickel positive electrode material. During the battery cycle, the high-nickel positive electrode material will expand and shrink. The method provided by the present invention enables AlCl3 to have a good wrapping and solidification effect on the high-nickel positive electrode material, and at the same time effectively prevents γ-Al2O3 from falling off from the high-nickel positive electrode material due to the expansion and contraction of the high-nickel positive electrode material.

[0057] As can be seen from the above, the above-mentioned preparation method provided by the embodiment of the present invention, by utilizing the organic-inorganic interface, is quickly, efficiently and controllably prepared in one step a high-nickel positive electrode material with low residual alkali and undamaged high-nickel positive electrode material structure. The complexity of the traditional water washing process, which repeatedly adjusts the water-to-material ratio, water washing time, stirring intensity and water temperature through orthogonal experiments, is reduced, and the uncontrollability of the high-nickel positive electrode material in contact with water during the process of feeding, discharging, filtering and drying is also reduced, which greatly reduces the uncontrollable factors, reduces the experimental intensity, shortens the experimental cycle, and improves production efficiency. AlCl3 fixes porous γ-Al2O3 particles on the surface of the high-nickel positive electrode material in the form of a film, so that the porous γ-Al2O3 particles on the surface of the high-nickel positive electrode material are not easy to fall off. The method is simple to operate and has the potential for large-scale promotion.

[0058] In a third aspect, an embodiment of the present invention provides a lithium battery, wherein the positive electrode of the lithium battery includes the above-mentioned low residual alkali and high nickel positive electrode material.

[0059] The present invention will be further described below in conjunction with the embodiments.

[0060] A method for preparing a low-residual-alkali high-nickel positive electrode material comprises the following steps:

[0061] Step 1: Evenly mix the high-nickel precursor, lithium hydroxide, lithium carbonate, etc. and then sinter to prepare the high-nickel positive electrode material S1.

[0062] Step 2: Add the high nickel cathode material S1 obtained in step 1 to an organic solvent to obtain a mixed solution, and control the solid content to 10%-70%. At a low speed, control the high nickel cathode material to have no precipitation, and the thickness of the supernatant of the mixed solution is greater than 0.

[0063] Step 3: Start stirring, add water to the mixed solution obtained in step 2, and control the ratio of water: high-nickel positive electrode material to 0.5-30. Increase the stirring intensity, use the stirring paddle to drive the high-nickel positive electrode material to move upward and contact with water to wash away the residual alkali, and the high-nickel positive electrode material uses its own gravity to move downward and separate from contact with water. At the same time, use an organic solvent to isolate the high-nickel positive electrode material and water, protect the high-nickel positive electrode material from excessive washing with water, resulting in excessive lithium removal and structural changes, and prevent internal lithium from migrating to the outside. Turn on the online pH value to monitor the pH changes in the water in real time, using the formula:

[0064] “J 水洗后高镍正极材料残碱 =J 高镍正极材料初始残碱 -J 水溶剂碱 ”

[0065] Calculate and determine the residual alkali content of high-nickel positive electrode material in the solution, where J 水溶剂碱 Use an online pH monitoring system to detect. When the pH reaches the target value, reduce the stirring intensity to allow the high-nickel positive electrode material to sink and separate from the water.

[0066] Take samples to test the residual alkali of the high-nickel positive electrode material. If the residual alkali value of the high-nickel positive electrode material is unqualified, continue step 3 until the residual alkali of the high-nickel positive electrode material is qualified.

[0067] Step 4: After the residual alkali value of the high-nickel positive electrode material obtained in step 3 is qualified, add NaAlO2 solution to the solution in step 3, use the aqueous solution to wash the residual alkali to slowly produce Al(OH)3 and precipitate it on the surface of the high-nickel positive electrode material, control the NaAlO2 addition rate to control the slow and uniform precipitation of Al(OH)3 and adsorption on the surface of the high-nickel positive electrode material, and control the molar ratio of Al in NaAlO2: high-nickel positive electrode material to be 0.005%-2%. After the precipitation of Al(OH)3 is completed, add AlCl3 solution to the organic solvent in the lower layer, control the molar ratio of AlCl3: high-nickel positive electrode material to be 0.005%-2%, mix for 1 hour, separate the solid and liquid, filter, and obtain the coated precursor S2.

[0068] Step 5: Sinter the coated precursor S2 obtained in step 4 at 150℃-300℃ in an oxygen atmosphere for 2-10h to obtain a crude product S3, control the heating and cooling rate to 3℃ / min, and after cooling to ≤80℃, take it out, grind and sieve it to obtain a finished product of low residual alkali and high nickel positive electrode material.

[0069] Example 1

[0070] A method for preparing a low-residual-alkali high-nickel positive electrode material comprises the following steps:

[0071] The precursor Ni 0.92 Co 0.08 Mn 0.02 After the mixture is uniformly mixed with lithium hydroxide, it is sintered in 99% oxygen at 550°C for 2 hours and at 710°C for 12 hours, wherein the heating rate and cooling rate are controlled at 3°C / min. When the temperature drops below 100°C, the intermediate product S1 (also called first sintering material) is obtained by grinding and sieving.

[0072] Add 20kg of intermediate S1 to 40L of carbon tetrachloride solution, stir at 100rpm, then add 40L of water; increase the stirring intensity to 200rpm, monitor the pH change in water in real time with online pH value, when the pH value reaches 12.96, reduce the stirring to 100rpm, take samples to detect the residual alkali of high-nickel positive electrode material, and after the residual alkali of the test product is lower than 4000ppm, add 2L1mol / LNaAlO2 to the solution at a uniform rate within 0.5h. Continue stirring for 0.5h, remove the supernatant, add 2L1mol / LAlCl3 / carbon tetrachloride solution to the mixed solvent, filter the mixed solution of high-nickel positive electrode material and organic solvent, and dry at 120℃ for 2h to obtain the coated precursor S2.

[0073] The coated precursor S2 was sintered at 200°C for 5h to obtain the crude product S3, and the heating and cooling rate was controlled to be 3°C / min. After the temperature dropped to ≤80°C, the crude product was taken out, ground and sieved to obtain a finished product of low residual alkali and high nickel positive electrode material.

[0074] Example 2

[0075] A method for preparing a low-residual-alkali high-nickel positive electrode material comprises the following steps:

[0076] Ni 0.95 Co 0.03 Mn 0.02 After the mixture is uniformly mixed with lithium hydroxide, it is sintered in 99% oxygen at 550°C for 2 hours and at 700°C for 12 hours, wherein the heating rate and cooling rate are controlled at 3°C / min. When the temperature drops below 100°C, the intermediate product S1 (also called first sintering material) is obtained by grinding and sieving.

[0077] Add 15kg of intermediate S1 to 30L of carbon tetrachloride solution, stir at 100rpm, then add 30L of water; increase the stirring intensity to 200rpm, and use the online pH monitoring system to monitor the pH change in the water in real time. When the pH value reaches 13.03, reduce the stirring speed to 100rpm, take samples to detect the residual alkali of the high-nickel cathode material, and after the residual alkali of the test product is less than 5000ppm, add 2L1mol / LNaAlO2 to the solution at a uniform rate within 0.5h. Continue stirring for 0.5h, remove the supernatant, add 2L1mol / LAlCl3 / carbon tetrachloride solution to the mixed solvent, filter the mixed solution of the high-nickel cathode material and the organic solvent, and dry at 120℃ for 2h to obtain the coated precursor S2.

[0078] The coated precursor S2 was sintered at 250°C for 5h to obtain the crude product S3, and the heating and cooling rate was controlled to be 3°C / min. After the temperature dropped to ≤80°C, the crude product was taken out, ground and sieved to obtain a finished product of low residual alkali and high nickel positive electrode material.

[0079] Comparative Example 1-Comparative Example 4:

[0080] The precursor Ni 0.92 Co 0.08 Mn 0.02 After the mixture is uniformly mixed with lithium hydroxide, it is sintered in 99% oxygen at 550°C for 2 hours and at 710°C for 12 hours, wherein the heating rate and cooling rate are controlled at 3°C / min. When the temperature drops below 100°C, the intermediate product S1 is obtained by grinding and sieving.

[0081] 20 kg of intermediate S1 was added to 40 L of water, and the stirring intensity was 200 rpm. The stirring time was 5 min, 10 min, 15 min, and 20 min respectively. After stirring, 2 L of 1 mol / L NaAlO was added simultaneously. 2。Subsequently, the coated precursors S2-1, S2-2, S2-3 and S2-4 were obtained by filtration and drying at 120°C for 2h. The coated precursors S2-1, S2-2, S2-3 and S2-4 were sintered at 400°C for 5h to obtain the high-nickel positive electrode material finished coated precursors S3-1, S3-2, S3-3 and S3-4. The heating and cooling rate was controlled to be 3°C / min. After the temperature dropped to ≤80°C, the products were taken out, ground and sieved to obtain the finished products.

[0082] Comparative Example 5

[0083] The precursor Ni 0.92 Co 0.08 Mn 0.02 After the mixture is uniformly mixed with lithium hydroxide, it is sintered in 99% oxygen at 550°C for 2 hours and at 710°C for 12 hours, wherein the heating rate and cooling rate are controlled at 3°C / min. When the temperature drops below 100°C, the intermediate product S1 (also called first sintering material) is obtained by grinding and sieving.

[0084] Add 20kg of intermediate S1 to 40L of carbon tetrachloride solution, stir at 100rpm, then add 40L of water; increase the stirring intensity to 200rpm, monitor the pH change in water in real time with online pH value, when the pH value reaches 12.96, reduce the stirring to 100rpm, take samples to detect the residual alkali of high-nickel positive electrode material, and after the residual alkali of the test product is lower than 4000ppm, add 2L1mol / LNaAlO2 to the solution at a uniform rate within 0.5h. Continue stirring for 0.5h, remove the supernatant, filter the mixed solution of high-nickel positive electrode material and organic solvent, and dry at 120℃ for 2h to obtain the coated precursor S2.

[0085] The coated precursor S2 was sintered at 200°C for 5h to obtain the crude product S3, and the heating and cooling rate was controlled to be 3°C / min. After the temperature dropped to ≤80°C, the crude product was taken out, ground and sieved to obtain a finished product of low residual alkali and high nickel positive electrode material.

[0086] Comparative Example 6

[0087] A method for preparing a low-residual-alkali high-nickel positive electrode material comprises the following steps:

[0088] The precursor Ni 0.92 Co 0.08 Mn 0.02 After the mixture is uniformly mixed with lithium hydroxide, it is sintered in 99% oxygen at 550°C for 2 hours and at 710°C for 12 hours, wherein the heating rate and cooling rate are controlled at 3°C / min. When the temperature drops below 100°C, the intermediate product S1 (also called first sintering material) is obtained by grinding and sieving.

[0089] Add 20kg of intermediate S1 to 40L of carbon tetrachloride solution, stir at 100rpm, then add 40L of water; increase the stirring intensity to 200rpm, monitor the pH change in water in real time with online pH value, when the pH value reaches 12.96, reduce the stirring to 100rpm, take samples to detect the residual alkali of high-nickel cathode material, and stir at a constant speed for 0.5h after the residual alkali of the test product is less than 4000ppm. Continue stirring for 0.5h, remove the supernatant, add 2L1mol / LAlCl3 / carbon tetrachloride solution to the mixed solvent, filter the mixed solution of high-nickel cathode material and organic solvent, and dry at 120℃ for 2h to obtain the coated precursor S2.

[0090] The coated precursor S2 was sintered at 200°C for 5h to obtain the crude product S3, and the heating and cooling rate was controlled to be 3°C / min. After the temperature dropped to ≤80°C, the crude product was taken out, ground and sieved to obtain a finished product of low residual alkali and high nickel positive electrode material.

[0091] The products obtained in Examples 1 to 2 and the products obtained in Comparative Examples 1 to 6 were respectively mixed with a conductive agent (SuperC) and a binder (PVDF) at a mass ratio of 80:10:10, and the corresponding mass of the materials was weighed and evenly mixed in a homogenizer to prepare a slurry, and the solid content was controlled to be 20-50%. The slurry was evenly coated on a 20μm aluminum foil using a coating machine, and the coating thickness was 0.25mm. After the pole piece was dried and rolled, a positive pole piece with a diameter of 12mm was prepared. Metal lithium was used as the negative electrode, and a CR2032 button cell was assembled using a LiPF6 / EC / EMC electrolyte and a PE separator.

[0092] Cycle test: After the button cell was placed for 10 hours, it was placed on a blue battery tester (CT2001C) for charge and discharge cycle performance test. The test conditions were set as: 25°C, 2.8-4.3V, 1C=200mAhg -1 , 0.1C / 0.1C button half-cell test 3 cycles, 1C / 1C cycle 100 weeks, the specific capacity and cycle performance of the products prepared in Examples 1 to 2 and the products prepared in Comparative Examples 1 to 6 were investigated. The specific electrochemical properties are shown in Table 1 below:

[0093] Table 1

[0094]

[0095]

[0096] It can be seen from Table 1 above that after removing residual alkali and double coating through this technology, the capacity and rate are significantly improved, and the capacity retention rate is significantly improved.

[0097] The following Table 2 shows the results of surface residual alkali detection of the products prepared in Examples 1-2 and Comparative Examples 5-6 at different stirring times.

[0098] Table 2

[0099]

[0100] It can be seen from Table 2 above that as the stirring time increases, the residual alkali content on the surface of the high-nickel positive electrode material gradually decreases.

[0101] The following Table 3 shows the surface residual alkali detection results of the products obtained in Examples 1-2 and Comparative Examples 1-6.

[0102] Table 3

[0103] sample LiOH% <![CDATA[Li2CO3%]]> Residual alkali ppm Example 1 2322 1190 3512 Example 2 2760 1805 4345 Comparative Example 1 4815 3590 8405 Comparative Example 2 2576 2012 4588 Comparative Example 3 2595 1300 3895 Comparative Example 4 2045 980 3025 Comparative Example 5 2355 1250 3605 Comparative Example 6 2305 1170 3475

[0104] It can be seen from the above Table 3: For Comparative Examples 1-4, the traditional water washing method can reduce the residual alkali value by increasing the water washing time, but the high nickel positive electrode material is always in contact with water while the time is extended. It can be seen from Table 1 that the capacity, especially the rate and cycle performance, are significantly reduced after the time is extended. This is because the high nickel positive electrode material is in contact with water for a long time, and the lattice lithium in the high nickel positive electrode material is inevitably precipitated, resulting in an inevitable decrease in the rate and cycle. It can be seen from Comparative Examples 5 and 6 that the rear-end coating has little effect on the residual alkali, but combined with Table 1, single coating Al2O3 or AlCl3, the cycle performance and rate are improved to varying degrees, but it is lower than the effect of double coating of porous Al2O3 particles combined with AlCl3 film.

[0105] In summary, the solution provided by the embodiment of the present invention uses an organic solvent to isolate the effective contact time between water and high-nickel positive electrode materials to prevent lattice lithium from washing out, and the porous Al2O3 isolates the electrolyte while providing a lithium ion transmission channel, and the AlCL3 film can further isolate the contact between the electrolyte and the high-nickel positive electrode material during the cycle to reduce the occurrence of side reactions, while controlling the AlCL3 coating amount to control the film thickness and thus reduce the impact on lithium ion transmission. After the above treatment, a low residual alkali high nickel positive electrode material with low residual alkali value, improved capacity, rate and cycle can be obtained.

[0106] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A low residual alkali high nickel positive electrode material, characterized in that: It includes a substrate and a coating layer on the surface of the substrate, the substrate is a high-nickel positive electrode material, the coating layer includes an AlCl3 layer and porous γ-Al2O3 particles embedded in the AlCl3 layer, and at least part of the porous γ-Al2O3 particles are in contact with the high-nickel positive electrode material.

2. The low residual alkali high nickel positive electrode material according to claim 1, characterized in that: The chemical formula of the high nickel cathode material is LiNi x M 1-x O2, wherein 0.6≤x≤1.0, and M is selected from at least one of Co, Mn, and Al.

3. The low residual alkali high nickel positive electrode material according to claim 1 or 2, characterized in that: The thickness of the coating layer on the surface of the low-residual-alkali-high-nickel positive electrode material is 0.5nm-50nm.

4. A method for preparing a low residual alkali high nickel positive electrode material according to any one of claims 1 to 3, characterized in that: include: Water is added to an organic solvent containing the high-nickel positive electrode material to obtain a dispersed system of an upper aqueous phase and a lower organic phase; the high-nickel positive electrode material is moved upward into the upper aqueous phase by stirring, and the residual alkali on the surface of the high-nickel positive electrode material is removed by washing with water; Al(OH)3 is deposited and adsorbed on the surface of the high-nickel positive electrode material, and the high-nickel positive electrode material is then coated with AlCl3; and finally, low-temperature sintering is performed to obtain the low residual alkali high-nickel positive electrode material.

5. The preparation method according to claim 4, characterized in that: The following steps are involved: The high-nickel positive electrode material is mixed with the organic solvent, stirred at a low speed, and then the water is added to obtain a dispersion system of an upper aqueous phase and a lower organic phase; Increasing the stirring speed to make the high-nickel positive electrode material in the dispersed system contact with the upper aqueous phase to wash away the residual alkali on the surface of the high-nickel positive electrode material, and then reducing the stirring speed to make the high-nickel positive electrode material sink into the lower organic phase to obtain a mixed solution with qualified residual alkali on the surface of the high-nickel positive electrode material; Depositing and adsorbing Al(OH)3 on the surface of the high-nickel positive electrode material, adding AlCl3 solution to the lower organic phase, and collecting the solid by solid-liquid separation to obtain a coating precursor; The coated precursor is sintered at low temperature to obtain the low residual alkali and high nickel positive electrode material.

6. The preparation method according to claim 5, characterized in that: The preparation of the dispersion system comprises: mixing the high-nickel positive electrode material with the organic solvent, stirring at a low speed, and then adding water to obtain a dispersion system of an upper aqueous phase and a lower organic phase; Preferably, the organic solvent includes one or more of chloroform, carbon tetrachloride, ethylene dichloride, dibromomethane, bromoform, chlorobenzene, and carbon disulfide; Preferably, the solid content in the dispersed system is 10%-70%; Preferably, the stirring speed of the low-speed stirring is 0-150 rpm.

7. The preparation method according to claim 5, characterized in that: The preparation of the mixed solution comprises: increasing the stirring speed of the dispersed system, and under high-speed stirring conditions, allowing the high-nickel positive electrode material to move upward and contact the water to wash away residual alkali, and an online pH value monitoring system to monitor the pH change in the water in real time, and when the pH reaches the target value, reducing the stirring speed to allow the high-nickel positive electrode material to sink and separate from the water; Preferably, the ratio of the water to the high-nickel positive electrode material is controlled to be 0.5 to 30; Preferably, the stirring speed of the high-speed stirring is 200-500 rpm, and the stirring speed of the low-speed stirring is 0-150 rpm; Preferably, the formula is used: 水洗后高镍正极材料的表面残碱 =J 高镍正极材料初始残碱 -J 水溶剂碱 ” Calculate and determine the surface residual alkali content of the high nickel positive electrode material in the solution, where: J 水溶剂碱 Detection using an online pH monitoring system; Preferably, sampling is performed to detect the residual alkali content on the surface of the high-nickel positive electrode material. If the residual alkali content on the surface of the high-nickel positive electrode material is unqualified, stirring and monitoring are continued until the residual alkali content on the surface of the high-nickel positive electrode material is qualified.

8. The preparation method according to claim 5, characterized in that: The preparation of the coating precursor comprises: adding aluminate to the mixed solution, allowing Al(OH)3 produced by hydrolysis of the aluminate to precipitate and adsorb to the surface of the high-nickel positive electrode material, after the precipitation of Al(OH)3 is completed, extracting the supernatant, adding AlCl3 solution, and collecting the solid by solid-liquid separation to obtain the coating precursor; Preferably, the metaaluminate includes one or more of NaAlO2 and KAlO2; Preferably, the molar ratio of Al in the metaaluminate to the high-nickel positive electrode material is controlled to be 0.005%-2%; Preferably, the molar ratio of AlCl3 in the AlCl3 solution to the high-nickel positive electrode material is controlled to be 0.005%-2%; Preferably, after the Al(OH)3 precipitation is completed, the supernatant is extracted, the AlCl3 solution is added, and after mixing for 1 hour, the solid is collected by solid-liquid separation to obtain a coating precursor.

9. The preparation method according to claim 5, characterized in that: The preparation of the low residual alkali high nickel positive electrode material comprises: sintering the coated precursor at 150° C.-300° C. for 2 h-10 h to obtain a crude product; Preferably, sintering is carried out in an oxygen atmosphere, and the oxygen concentration is ≥ 99%; Preferably, the method further comprises: cooling the crude product to below 80° C., taking it out, grinding and screening it, and obtaining a finished product of a low-residual-alkali and high-nickel positive electrode material; Preferably, the heating rate and the cooling rate are both controlled to be 3°C / min.

10. A lithium battery, characterized in that: The lithium battery positive electrode comprises the low residual alkali high nickel positive electrode material according to any one of claims 1 to 3 or the low residual alkali high nickel positive electrode material prepared by the preparation method according to any one of claims 4 to 9.

Citation Information

Patent Citations

  • Method for aluminum cladding of positive electrode material by wet method, positive electrode material, positive electrode and battery

    CN105845926A

  • Preparation method of high-nickel positive electrode material with low residual alkali, high compaction and uniform coating layer

    CN112194200A

  • Preparation method of high-nickel positive electrode material of composite coating layer

    CN112310376A

  • Method for improving rate capability of solid-state lithium battery

    CN112421127A

  • Coating method for improving thermal stability of high-nickel positive electrode material

    CN114335549A

Cited By

  • Positive electrode material, preparation method and device thereof and lithium ion battery

    CN119400845A

  • Ternary positive electrode slurry as well as preparation method and application thereof

    CN120767291A