Three-dimensional porous graphite current collector for preparing ultrathin lithium composite electrode, preparation method and application

Through the preparation of three-dimensional porous graphite current collector, the lithium-philicity and lithium-embedded compound structure of graphite are used to solve the problems of uneven deposition and mechanical strength of ultra-thin lithium belts, and high specific capacity and electrochemical stability are achieved, which is suitable for high-specificity Energy battery requirements.

CN119050373APending Publication Date: 2024-11-29JILIN UNIVERSITY

Patent Information

Application Number
CN202411180393.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

现有超薄锂带在沉积/剥离过程中不均匀沉积导致锂枝晶形成,导致电池库仑效率低、容量衰减快、消耗电解液和安全问题,且机械强度和可加工性差,难以制备薄锂 带。

Method used

The ultrathin lithium composite electrode is prepared by roll pressure regulating thickness. The lithium-embedded compound of graphite is lithium-philic, inducing lithium ions into pore deposition, alleviating the growth of lithium dendrites, and preparing ultra-thin through electrochemical prelithiation Thin lithium composite electrode.

Benefits of technology

It achieves high-quality specific capacity, inhibits the growth of lithium dendrites, improves electrochemical stability, simplifies the preparation process, reduces costs, is suitable for large-scale production, and meets the needs of high-specific energy batteries in the future.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050373A_ABST
    Figure CN119050373A_ABST
Patent Text Reader

Abstract

The invention discloses a three-dimensional porous graphite current collector for preparing an ultrathin lithium composite electrode, a preparation method and application, and belongs to the technical field of lithium metal batteries, and the method comprises the following steps: preparing the three-dimensional porous graphite current collector by adopting a freeze drying technology, and then adjusting the thickness of the three-dimensional porous graphite current collector by using a roller press to obtain the ultrathin lithium composite electrode. And finally, preparing the ultrathin lithium composite electrode by adopting an electrochemical pre-lithiation method and applying the ultrathin lithium composite electrode to a lithium metal battery. The thickness of the three-dimensional porous graphite current collector can be regulated and controlled through rolling to prepare the ultrathin lithium composite electrode; due to the characteristic of light weight, the ultrathin lithium composite electrode can realize relatively high mass specific capacity, and can meet the requirements of practical high-specific-energy batteries in the future; the lithium intercalation compound of the graphite has good lithium affinity, and lithium can be intercalated by utilizing the graphite to prepare the three-dimensional skeleton, so that skeleton ion transmission is realized; a lithium intercalation compound of graphite is used as a lithium-loving site, lithium ions are induced to enter pores for deposition, and top growth of lithium dendrites is further relieved. The three-dimensional porous graphite current collector is applied to preparation of an ultrathin lithium composite electrode, the process is simple, the cost is low, and large-scale production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and in particular relates to a three-dimensional porous graphite current collector for ultra-thin lithium composite electrodes, and preparation and application thereof. Background Art

[0002] With the rapid development of electrification in the transportation and new energy industries, people have put forward higher requirements for batteries in terms of energy density and power density, safety of use and portability. Lithium metal is expected to be used as a negative electrode material in the next generation of high specific energy secondary battery systems due to its high theoretical mass specific capacity, low electrochemical potential, near-minimum solid density (lightweight), and small atomic radius. However, thick lithium sheets (e.g., 600 μm thick, 120 mAh cm –2 ) as the negative electrode, excessive metallic lithium seriously reduces the battery energy density and causes a waste of lithium resources. In practical applications, in order to further improve the utilization rate of active materials, increase the overall energy density of the battery, and meet the needs of future practical high-energy-density batteries, the lithium metal negative electrode needs to use an ultra-thin lithium negative electrode.

[0003] However, ultra-thin lithium negative electrodes face the problem of uneven deposition during deposition / stripping, and the unevenness of lithium will lead to the formation of lithium dendrites. The existence of lithium dendrites is one of the major obstacles to the development of metal lithium batteries, which causes low coulombic efficiency of the battery, rapid capacity decay, electrolyte consumption and safety issues. In addition, metallic lithium exhibits obvious diffusion creep and processing viscosity, resulting in a sharp drop in the mechanical strength and processability of ultra-thin lithium at room temperature, and it is difficult to prepare thin lithium strips by simple mechanical rolling methods. Therefore, the electrochemical instability and difficulty of preparation of ultra-thin lithium strips limit their application in lithium metal batteries.

[0004] The researchers considered that the above problems could be solved by preparing a three-dimensional current collector. The three-dimensional current collector is prepared by electrochemical pre-lithiation or melt lithium filling to prepare ultra-thin lithium metal electrodes. At the same time, due to its large specific surface area and suitable porosity, it not only provides effective support and adhesion for lithium metal, but also alleviates the volume expansion of lithium metal electrodes during repeated deposition and stripping, and slows down the growth rate of dendrites.

[0005] The prior art discloses a method for preparing a three-dimensional porous copper / lithium sulfide / metal lithium composite metal lithium negative electrode. The composite metal lithium negative electrode has a continuous three-dimensional pore structure, which can slow down the volume change of the metal lithium negative electrode during the charge and discharge process, increase the specific surface area of ​​the electrode, and reduce the local current density of the electrode, thereby inhibiting the generation of lithium dendrites. However, the solid density of the metal skeleton itself is high, which seriously weakens the density advantage of the lithium metal negative electrode itself in terms of energy density. The prior art also discloses a three-dimensional carbon material and a preparation method thereof, a metal lithium composite electrode and a preparation method thereof. The three-dimensional carbon material maintains the elasticity and three-dimensional skeleton structure of the sponge, has a certain conductivity, and also has a large specific surface area and rich void structure. After depositing metal lithium, it can achieve high current density and high surface capacity; however, due to the poor lithium affinity of the carbon material, it is difficult to ensure that lithium metal enters the three-dimensional skeleton for deposition, which is not conducive to alleviating the growth of lithium dendrites.

[0006] Therefore, there is still a need to explore a three-dimensional current collector that is simple to prepare, low-cost, has good lithium affinity and can adjust the thickness to prepare ultrathin lithium metal anode. Summary of the invention

[0007] In view of the problems of electrochemical instability and difficulty in preparation of existing ultra-thin lithium strips, the present invention provides a three-dimensional porous graphite current collector, preparation method and application for preparing ultra-thin lithium composite electrodes. The three-dimensional porous graphite current collector can be used to adjust the thickness of the ultra-thin lithium composite electrode by rolling; its light weight enables the ultra-thin lithium composite electrode to achieve a higher mass specific capacity, which can meet the needs of future practical high-energy-density batteries; the graphite lithium-intercalation compound has good lithium affinity, and the three-dimensional skeleton prepared by graphite itself can be intercalated with lithium to achieve skeleton ion transmission; the graphite lithium-intercalation compound acts as a lithium-affinity site to induce lithium ions to enter the pores for deposition, further alleviating the growth of lithium dendrite tops. The three-dimensional porous graphite current collector is applied to the preparation of ultra-thin lithium composite electrodes, which has a simple process, low cost and is conducive to large-scale production.

[0008] The present invention is achieved through the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode, which specifically comprises the following steps:

[0010] S1. Mix graphite, conductive agent Superp and binder CMCNa in a certain proportion, and then put them into a mortar for thorough grinding;

[0011] S2, adding water solvent to the mixture ground in step S1, and then stirring it evenly with a homogenizer to obtain a slurry;

[0012] S3, coating the slurry obtained in step S2 on a copper foil, then freezing it in liquid nitrogen, and then freezing it in a freeze dryer to obtain a three-dimensional porous graphite current collector;

[0013] S4. Using a roller press, adjust the thickness of the three-dimensional porous graphite current collector obtained in step S3.

[0014] Furthermore, in step S1, the mass ratio of graphite, conductive agent Superp, and binder CMCNa is 180-200 mg: 20-30 mg: 20-30 mg.

[0015] Furthermore, in step S2, the mass ratio of the water solvent to the graphite is 9:1 to 7:1.

[0016] Furthermore, in step S2, the rotation speed of the homogenizer is 2000 r / min, and the use time of the homogenizer is 20 to 30 min.

[0017] Furthermore, in step S3, the copper foil is washed 1 to 3 times with ethanol to clean surface impurities.

[0018] Furthermore, in step S3, the slurry coating thickness is 100-200 μm.

[0019] Furthermore, in step S3, the graphite slurry coated on the copper foil is frozen in a liquid nitrogen environment for 1 to 3 minutes.

[0020] Furthermore, in step S3, the freeze-drying treatment time in the freeze dryer is 6 to 9 hours.

[0021] Furthermore, in step S4, a roller press is used to adjust the thickness of the three-dimensional porous graphite current collector to 10 to 50 mm.

[0022] In a second aspect, the present invention provides a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode, which is prepared by the preparation method described in the first aspect.

[0023] In the third aspect, the present invention also provides an application of a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode in the preparation of an ultra-thin lithium composite electrode, specifically comprising: pre-lithiation of the three-dimensional porous graphite current collector to prepare an ultra-thin lithium composite electrode (3D-LiC6@Li); the prepared 3D-LiC6@Li is used as a negative electrode in a lithium metal battery.

[0024] Furthermore, the pre-lithiation treatment was carried out using a three-dimensional porous graphite current collector as the working electrode, a lithium sheet as the reference electrode and a counter electrode, and a lithium-sulfur electrolyte (1M LiTFSI in DME:DOL=1:1Vol% with 1%LiNO3) as the electrolyte at 1 mA cm -2Deposition was carried out at a current density of 1 to 10 h.

[0025] Compared with the prior art, the advantages of the present invention are as follows:

[0026] 1. The three-dimensional porous graphite current collector can be rolled to adjust the thickness and prepare an ultra-thin lithium metal composite negative electrode; graphite material has the characteristics of light weight, and when used as a three-dimensional current collector of lithium metal, it can enable the composite electrode to achieve a higher mass specific capacity. Therefore, the ultra-thin lithium composite electrode of the present invention can meet the needs of future practical high-energy-density batteries.

[0027] 2. The three-dimensional porous graphite current collector of the present invention is prepared by pre-lithiation to prepare an ultra-thin lithium composite electrode, which has a simple preparation process, low cost, and is conducive to large-scale production.

[0028] 3. The three-dimensional porous graphite current collector of the present invention has a large specific surface area and a rich pore structure, which can effectively reduce the actual current density and thus effectively inhibit dendrite growth.

[0029] 4. The prepared three-dimensional porous graphite current collector itself can embed lithium and realize skeleton ion transport; then the lithium embedding compound of graphite acts as a lithium-philic site to induce lithium ions to enter the pores and deposit, further alleviating the growth of the top of the lithium dendrite.

[0030] 5. The three-dimensional porous graphite prepared by the present invention can realize the mixed storage of graphite lithium embedding and lithium metal deposition. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0032] Figure 1 is a SEM image of the three-dimensional porous graphite current collector prepared in Example 1 of the present invention;

[0033] Among them, Figure a is a plan view of a three-dimensional porous graphite current collector, and Figure b is a cross-sectional view of a three-dimensional porous graphite current collector;

[0034] Figure 2 This is a hybrid energy storage mechanism diagram of the three-dimensional porous graphite current collector prepared in Example 1 of the present invention;

[0035] Figure 3 3. The three-dimensional porous graphite current collector prepared in Example 1 of the present invention has different energy storage stages.

[0036] Figure 4 is a SEM image of the ultra-thin lithium composite electrode obtained in Example 1 of the present invention;

[0037] Figure 5 : is a coulombic efficiency diagram of half-cells prepared in Examples 1 to 2 of the present invention and Comparative Examples 1 to 3;

[0038] Figure 6 This is a test diagram of nucleation overpotential of different current collectors prepared in Examples 1 to 2 of the present invention and Comparative Examples 1 to 3;

[0039] Figure 7 It is a full battery cycle curve diagram prepared by Examples 1-2 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION

[0040] In order to clearly and completely describe the technical solution and its specific working process of the present invention, the specific implementation methods of the present invention are as follows in conjunction with the accompanying drawings of the specification:

[0041] The present invention firstly adopts freeze-drying technology to prepare a three-dimensional graphite porous current collector, then uses a roller press to adjust the thickness of the three-dimensional porous graphite current collector, and finally adopts an electrochemical pre-lithiation method to prepare an ultra-thin lithium composite electrode for application in lithium metal batteries.

[0042] Example 1

[0043] This embodiment provides a method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode, which specifically includes the following steps:

[0044] (1) Weigh 190 mg of graphite, 25 mg of conductive agent Superp, and 25 mg of binder CMCNa respectively, mix them, put them into a mortar and grind them thoroughly;

[0045] (2) The ground mixture was added with 1500 μL of aqueous solvent, and then placed in a homogenizer and stirred at 2000 r / min for 20 min to obtain a slurry.

[0046] (3) The obtained slurry was coated on a copper foil with a coating thickness of 100 μm; then it was quickly placed in liquid nitrogen for freezing for 1 min, and then placed in a vacuum freeze dryer for 8 h for freeze drying to obtain a three-dimensional porous graphite current collector;

[0047] (4) using a roller press to adjust the thickness of the three-dimensional porous graphite current collector to 40 μm;

[0048] (5) The three-dimensional porous graphite current collector was used as the working electrode, the lithium sheet was used as the reference electrode and the counter electrode, and the electrolyte was 1MLiTFSI in DME:DOL=1:1Vol%with 1%LiNO3. -2 An ultrathin lithium composite electrode (3D-LiC6@Li) was prepared by deposition at a current density of 6 h.

[0049] Example 2

[0050] This embodiment provides a method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode, which specifically includes the following steps:

[0051] (1) Weigh 180 mg of graphite, 25 mg of conductive agent Superp, and 20 mg of binder CMCNa respectively, mix them, put them into a mortar and grind them thoroughly;

[0052] (2) adding 1450 μL of aqueous solvent to the above-mentioned ground mixture, and then placing it in a homogenizer, stirring at a speed of 2000 r / min for 25 min to obtain a slurry;

[0053] (3) The obtained slurry was coated on copper foil with a coating thickness of 150 μm. Then it was quickly placed in liquid nitrogen for freezing for 2 minutes, and then placed in a vacuum freeze dryer for 6 hours to obtain a three-dimensional porous graphite current collector;

[0054] (4) Using a roller press to adjust the thickness of the three-dimensional porous graphite current collector to 35 μm;

[0055] (5) The three-dimensional porous graphite current collector was used as the working electrode, the lithium sheet was used as the reference electrode and the counter electrode, and the electrolyte was 1MLiTFSI in DME:DOL=1:1Vol%with 1%LiNO3. -2 An ultrathin lithium composite electrode (3D-LiC6@Li) was prepared by deposition at a current density of 6 h.

[0056] Comparative Example 1:

[0057] This embodiment provides a method for preparing a lithium / copper foil composite electrode, which specifically includes the following steps:

[0058] (1) Conventional negative electrode current collector copper foil, not coated;

[0059] (2) The copper foil current collector was used as the working electrode, the lithium sheet was used as the reference electrode and the counter electrode, and the electrolyte was 1M LiTFSI in DME:DOL = 1:1 Vol% with 1% LiNO3 at 1 mA cm -2 The composite electrode was prepared by deposition at a current density of 6 h.

[0060] Comparative Example 2:

[0061] This embodiment provides a method for preparing a lithium / copper foam composite electrode, which specifically includes the following steps:

[0062] (1) Conventional negative electrode current collector copper foam, not coated;

[0063] (2) The copper foam current collector was used as the working electrode, the lithium sheet was used as the reference electrode and the counter electrode, and the electrolyte was 1MLiTFSI in DME:DOL=1:1Vol%with 1%LiNO3. -2 The composite electrode was prepared by deposition at a current density of 6 h.

[0064] Comparative Example 3:

[0065] This embodiment provides a method for preparing a lithium / two-dimensional graphite composite electrode, which specifically includes the following steps:

[0066] (1) Weigh 190 mg of graphite, 25 mg of conductive agent Superp, and 25 mg of binder CMCNa respectively, mix them, put them into a mortar and grind them thoroughly.

[0067] (2) The ground mixture was added with 1500 μL of aqueous solvent, and then placed in a homogenizer and stirred at 2000 r / min for 20 min to obtain a slurry.

[0068] (3) The obtained slurry was coated on a copper foil with a coating thickness of 100 μm, and then placed in an oven at 60° for 8 h to obtain a two-dimensional graphite current collector.

[0069] (4) Use a roller press to adjust the thickness of the two-dimensional graphite current collector to 36 μm.

[0070] (5) The two-dimensional graphite current collector was used as the working electrode, the lithium sheet was used as the reference electrode and the counter electrode, and the electrolyte was 1MLiTFSI in DME:DOL=1:1Vol%with 1%LiNO3. -2 The composite electrode was prepared by deposition at a current density of 6 h.

[0071] The current collectors obtained in Examples 1 to 2 and Comparative Examples 1 to 3 were used as positive electrodes, lithium sheets as negative electrodes, Celgard 2325 type separators, and 1M LiTFSI in DME:DO L=1:1 Vol% with 1% LiNO3 electrolytes were assembled into half cells for constant current charge and discharge performance tests.

[0072] from Figure 2 It can be seen from the capacity-voltage curve that at a current density of 1 mA cm -2 And when the capacity is 1 mAh, the graphite current collector of Example 1 exhibits mixed energy storage of graphite lithium insertion and lithium metal deposition.

[0073] from Figure 3The XRD test results further prove that the graphite current collector of Example 1 first performs only intercalation lithium energy storage and then performs lithium metal deposition energy storage.

[0074] from Figure 5 The cycling performance test shows that at a current density of 1 mA cm -2 and a capacity of 1 mAh cm -2 Under the condition of 1mA cm -2 At a current density of 1.547 W, the nucleation overpotential of lithium metal of different current collectors was tested at the tenth cycle. Figure 6 It can be seen that the three-dimensional graphite current collectors in Examples 1 to 2 have overpotentials of 12.7 mV and 11.4 mV, respectively, which are significantly lower than the current collectors in the three comparative examples.

[0075] The active material (LiFePO4), Super P, and PVDF were weighed in a mass ratio of 8:1:1 and fully ground and mixed. An appropriate amount of NMP solvent was added and stirred overnight to form a uniform slurry, which was applied on Al foil and vacuum dried at 60°C for about 8 hours to obtain a composite positive electrode material (LFP).

[0076] LFP was used as the positive electrode, the composite electrode obtained in Examples 1 to 2 and Comparative Examples 1 to 3 was used as the negative electrode, Celgard 2325 was used as the separator, 1M LiPF6 in DMC:EC:EMC=1:1:1Vol%with1%VC was used as the electrolyte, and a full battery was assembled to perform a constant current charge and discharge performance test at a 1C rate.

[0077] like Figure 7 As shown, at a 1C rate, the discharge specific capacity of the full batteries of Examples 1-2 during the cycle is significantly higher than that of Comparative Examples 1-3.

[0078] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0079] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0080] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode, characterized in that: The specific steps include: S1. Mix graphite, conductive agent Superp and binder CMCNa in a certain proportion, and then put them into a mortar for thorough grinding; S2, adding water solvent to the mixture ground in step S1, and then stirring it evenly with a homogenizer to obtain a slurry; S3, coating the slurry obtained in step S2 on a copper foil, then freezing it in liquid nitrogen, and then freezing it in a freeze dryer to obtain a three-dimensional porous graphite current collector; S4. Using a roller press, adjust the thickness of the three-dimensional porous graphite current collector obtained in step S3.

2. A method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode according to claim 1, characterized in that: In step S1, the mass ratio of graphite, conductive agent Superp, and binder CMCNa is 180-200 mg: 20-30 mg: 20-30 mg.

3. The method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode according to claim 1, characterized in that: In step S2, the mass ratio of the water solvent to the graphite is 9:1 to 7:

1.

4. The method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode according to claim 1, characterized in that: In step S2, the speed of the homogenizer is 2000 r / min, and the homogenizer is used for 20 to 30 minutes.

5. The method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode according to claim 1, characterized in that: In step S3, the copper foil is washed with ethanol for 1 to 3 times to clean the surface impurities; the thickness of the slurry coating is 100 to 200 μm; the graphite slurry coated on the copper foil is frozen in a liquid nitrogen environment for 1 to 3 minutes.

6. The method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode according to claim 1, characterized in that: In step S3, the freeze-drying treatment time in the freeze dryer is 6 to 9 hours.

7. The method for preparing a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode according to claim 1, characterized in that: In step S3, a roller press is used to adjust the thickness of the three-dimensional porous graphite current collector to 10-50 mm.

8. A three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode, characterized in that: The method is prepared by any one of claims 1 to 7.

9. The use of a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode as claimed in claim 8 in preparing an ultra-thin lithium composite electrode, characterized in that: Specifically include: The three-dimensional porous graphite current collector is pre-lithiated to prepare an ultra-thin lithium composite electrode 3D-LiC6@Li; the prepared 3D-LiC6@Li is used as a negative electrode in lithium metal batteries.

10. The use of a three-dimensional porous graphite current collector for preparing an ultra-thin lithium composite electrode as claimed in claim 9 in preparing an ultra-thin lithium composite electrode, characterized in that: The pre-lithiation treatment uses a three-dimensional porous graphite current collector as the working electrode, a lithium sheet as the reference electrode and a counter electrode, and a lithium-sulfur electrolyte at 1 mA cm -2 Deposition was carried out at a current density of 1 to 10 h.

Citation Information

Patent Citations

  • Preparation method of porous electrode

    CN103943377A

  • Lithium metal secondary battery anode current collector and preparation method thereof

    CN110993954A

  • Graphene aerogel / metal lithium composite negative electrode material and preparation method thereof

    CN111048750A

  • Flexible self-supporting stainless steel mesh / graphene / lithium composite negative electrode and preparation method thereof

    CN111224069A

  • Prepatation of materials for energy storage devices using monolithic 3 dimensional of reduced graphene oxide and fabrication method thereby

    KR1020160027768A

Cited By

  • Negative current collector of negative-electrode-free lithium battery and preparation method of negative current collector

    CN120341292A

  • Negative current collector for a lithium battery without negative electrode and method for manufacturing the same

    CN120341292B

  • Preparation method and application of ultra-light conductive gradient porous composite current collector composed of nanofibers with wrinkled surfaces

    CN120784380A