Atomizing core, atomizer and electronic atomizing device

By using a combination of porous glass ceramic matrix and metal heating film, the tortuosity is controlled, and the problem of poor oil conduction effect of existing ceramic materials is solved, and more efficient atomization medium flow and better oil conduction effect are achieved, and electronics are extended. The service life of the smoke.

CN119054964APending Publication Date: 2024-12-03SMOORE INTERNATIONAL HOLDINGS LIMITED
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310646117.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The pore structure of the atomized core of the existing porous ceramic materials has poor controllability, resulting in poor oil conduction effect.

Method used

The porous glass ceramic matrix is ​​used to control its tortuosity between 1-2.5, and combined with the metal heating film, the atomized core is formed to improve the flow time and oil conduction effect of the atomized medium.

Benefits of technology

Under the same capillary force, the flow time of the atomized medium is shortened, the oil conduction effect is improved, the burnt smell and excessive smoke and stain caused by local high temperatures are avoided, and the service life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054964A_ABST
    Figure CN119054964A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic atomization, in particular to an atomization core, an atomizer and an electronic atomization device. The invention provides an atomizing core, the atomizing core comprises a porous matrix and a heating body, the porous matrix is a porous glass ceramic matrix, and the tortuosity of the porous glass ceramic matrix is 1-2.5. The tortuosity of the porous glass ceramic matrix is controlled to be 1-2.5, the through hole path is relatively short, and the oil guide effect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic atomization, and in particular to an atomization core, an atomizer and an electronic atomization device. Background Art

[0002] As a good substitute for traditional cigarettes, common e-cigarettes with e-liquid are generally composed of three parts: a cigarette rod, an atomizer core and an atomizer chamber. The battery is set in the cigarette rod, and the atomizer core is set in the e-liquid chamber. Among them, the atomizer core is the heart of the entire e-cigarette. The e-liquid is atomized into smoke through the atomizer core, and the atomized gas is exported to the mouthpiece. Compared with traditional cigarettes, the advantage of e-cigarettes is that they reduce harmful substances such as tar and CO in the smoke, and finally achieve the purpose of replacing cigarettes or relieving addiction, and reduce the absorption of harmful substances. The atomization method of the electronic cigarette atomization device currently on the market is mainly resistive heating atomization, which atomizes the electronic cigarette oil through the heat of the atomizer core. The atomizer core usually includes a porous matrix and a heating element. The existing porous matrix usually adopts materials with a porous structure such as cotton cores and porous ceramics to achieve the function of guiding the atomization medium to the heating element.

[0003] However, ceramic materials are usually prepared using complex components such as diatomaceous earth, and the porous matrix prepared therefrom has problems such as poor controllability of pore structure and poor oil conduction effect. Summary of the invention

[0004] The purpose of the present invention is to overcome the defect that the pores of the atomization core made of the existing porous ceramic material have poor oil conduction effect, and further provide an atomization core, an atomizer and an electronic atomization device.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme:

[0006] The present invention provides an atomizer core, which comprises a porous substrate and a heating element. The porous substrate is a porous glass ceramic substrate, and the tortuosity of the porous glass ceramic substrate is 1-2.5.

[0007] Preferably, the tortuosity of the porous glass-ceramic matrix is ​​1-2.

[0008] Preferably, the tortuosity of the porous glass-ceramic substrate is 1.3-1.9.

[0009] Tortuosity is also called tortuosity factor, also known as tortuosity, tortuosity, which means: the ratio of the "effective average path length" in the porous medium to the shortest distance measured along the macroscopic seepage direction; that is, it is defined as Where L tis the true length of the curved path; L0 is the straight length of the medium (the shortest macroscopic length); τ is the tortuosity. Due to the complex shape of the capillary, the flow of the fluid in the porous medium does not proceed in a straight line, but flows forward in a tortuous manner. The tortuosity reflects the degree of this tortuosity.

[0010] Preferably, the porosity of the porous glass-ceramic matrix is ​​greater than 50%;

[0011] Optionally, the porosity of the porous glass-ceramic matrix is ​​60-80%.

[0012] Preferably, the average pore size of the porous glass-ceramic matrix is ​​15-45 μm.

[0013] Preferably, the porous glass-ceramic matrix comprises pores formed by openings of glass-ceramic bubbles.

[0014] Optionally, the porous glass-ceramic matrix further includes pores formed by a pore former.

[0015] Preferably, the heating element is a metal heating film;

[0016] The heating element is arranged on at least one surface of the porous glass-ceramic substrate.

[0017] Preferably, the metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

[0018] The present invention provides an atomizer, wherein the atomizer comprises the atomizing core described above.

[0019] The present invention also provides an electronic atomization device, which includes the atomizer described above and a battery assembly.

[0020] Beneficial effects of the present invention:

[0021] The atomizer core provided by the present invention comprises a porous substrate and a heating element. The porous substrate adopts a porous glass-ceramic substrate, and the tortuosity of the porous glass-ceramic substrate is controlled to be 1-2.5. It is found through research that the porous glass-ceramic substrate under this specific tortuosity is conducive to shortening the overall flow time of the atomization medium and achieving a better oil conduction effect under the same capillary force and other factors. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 Comparison of smoke volume of the atomizer core bare chip in Example 2 of the present invention and Comparative Example 1 at different powers;

[0024] Figure 2 Atomizer core temperature curve diagram of Example 2 of the present invention;

[0025] Figure 3 Temperature field distribution diagram of the atomizer core of Example 2 of the present invention;

[0026] Figure 4 A diagram showing the deposition of soot on the atomizer core of Example 2 of the present invention after 300 puffs;

[0027] Figure 5 Schematic diagram of the atomizer of the present invention;

[0028] Figure 6 Schematic diagram of the electronic atomization device of the present invention;

[0029] Figure numerals: 1-atomizer, 2-battery assembly. DETAILED DESCRIPTION

[0030] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0031] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0032] The main atomization method of commercially available electronic cigarettes is resistive heating atomization, which atomizes the electronic cigarette oil by heating the atomizer core. Existing atomizer cores usually include a porous matrix and a heating element. The porous matrix usually uses materials with a porous structure such as cotton cores and porous ceramics to achieve the function of guiding the atomized medium to the heating element. However, ceramic materials are usually prepared using complex components such as diatomaceous earth, and the pore structure of the porous matrix prepared therefrom is poorly controllable and has a poor oil-conducting effect.

[0033] To this end, the present invention provides an atomizer core, which includes a porous matrix and a heating element; the porous matrix is ​​a porous glass-ceramic matrix, and the tortuosity of the porous glass-ceramic matrix is ​​1-2.5. The inventor found that the porous glass-ceramic matrix under this specific tortuosity has a relatively short through-hole path, which is conducive to making the overall flow time of the atomizing medium shorter and the oil guiding effect better under the same capillary force and other factors. At the same time, it further avoids the local high temperature of the atomizing surface caused by insufficient liquid supply, avoids the generation of burnt taste, and avoids the generation of excessive soot due to local high temperature, which can improve the taste and service life.

[0034] In some optional embodiments, the tortuosity of the porous glass-ceramic substrate can be 1, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, 1.21, 1.22, 1.23, 1.24, 1.25, 1.26, 1.27, 1.28, 1.29, 1.30, 1.31, 1.32, 1.33, 1.34, 1.35, 1.37, 1.39, 1.40, 1.42, 1.45, 1.47, 1.5, 1.52, 1.53, 1.55, 1.58, 1.60, 1.63, 1.65, 1.68, 1.70, 1.72, 1.75, 1.78 , 1.80, 1.84, 1.85, 1.87, 1.90, 1.94, 1.95, 1.98, 1.99, 2, 2.01, 2.02, 2.03, 2.04, 2.05, 2.06, 2.07, 2.08, 2.09, 2.10, 2.11, 2.12, 2.13, 2.14, 2.15, 2.16, 2.17, 2.18, 2.19, 2.20, 2.21, 2.22, 2.23, 2.24, 2.25, 2.26, 2.27, 2.28, 2.29, 2.30, 2.31, 2.32, 2.33, 2.34, 2.35, 2.36, 2.37, 2.38, 2.39, 2.40, 2.41, 2.42, 2.43, 2.44, 2.45, 2.46, 2.47, 2.48, 2.49, 2.5. Furthermore, the tortuosity of the porous glass-ceramic matrix is ​​1-2. Further, the tortuosity of the porous glass-ceramic matrix is ​​1.3-1.9. When the atomizer core and the atomizer are actually used, the user will not inhale all the time. During storage, too low tortuosity will cause the liquid atomization matrix to leak to the outside through the pores of the atomizer core, causing leakage problems. Therefore, appropriate tortuosity can take into account both the liquid conduction effect and the liquid locking effect, ensuring that there is no leakage during storage and improving the user experience.

[0035] In some optional embodiments, the porosity of the porous glass-ceramic matrix is ​​more than 50%. Optionally, the porosity of the porous glass-ceramic matrix is ​​60-80%. Among them, it includes pores formed by the openings of glass-ceramic bubbles. In other optional embodiments, the pores of the porous glass-ceramic matrix include pores formed by the openings of glass-ceramic bubbles, and also include pores formed by pore-forming agents. Further, in the porous glass-ceramic matrix, the pore volume formed by the openings of glass-ceramic bubbles accounts for more than 70% of the total pore volume of the porous glass-ceramic matrix. For example, it can be selected that the pore volume formed by the openings of the glass-ceramic bubbles accounts for 70.1%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or 100% of the total pore volume of the porous glass-ceramic matrix.

[0036] Porosity (volume porosity) is defined as the ratio of the total volume of pores in the porous glass-ceramic matrix to the volume of the porous glass-ceramic matrix.

[0037] In some optional embodiments, the average pore size of the porous glass-ceramic matrix is ​​15-45 μm. For example, the average pore size of the porous glass-ceramic matrix can be selected to be 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 26 μm, 27 μm, 28 μm, 29 μm, 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm, 38 μm, 39 μm, 40 μm, 41 μm, 42 μm, 43 μm, 44 μm, 45 μm.

[0038] In some optional embodiments, the heating element is a metal heating film; the heating element is arranged on at least one surface of the porous glass-ceramic substrate; further, the metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

[0039] In some optional embodiments, the preparation method of the heating element disposed on at least one surface of the porous glass-ceramic substrate includes at least one of printing, welding, evaporation, and deposition. For example, it is possible to print the heating element slurry on the substrate and sinter it at a preset temperature. It is possible to weld the heating element or heating net on the substrate. It is possible to evaporate / deposit the heating element on the substrate by physical vapor deposition (PVD) or chemical vapor deposition (CVD).

[0040] The atomizer core of the present invention can be obtained by conventional methods in the art, or by sintering glass ceramic bubbles. The glass ceramic bubbles are hollow structures, also known as hollow glass "microspheres", which can be obtained commercially. In some optional embodiments, the preparation method of the atomizer core obtained by sintering glass ceramic bubbles includes the following steps:

[0041] In some optional embodiments, the method for preparing the atomizer core comprises the following steps:

[0042] 1) mixing glass bubbles with a binder, a lubricant and water and extruding the mixture to obtain a green body;

[0043] 2) subjecting the green body in step 1) to a first sintering, a second sintering and a third sintering to obtain a porous glass-ceramic matrix;

[0044] 3) The raw material of the heating element is prepared on the porous glass ceramic substrate in step 2) and sintered into shape.

[0045] In some optional embodiments, in step 1): the binder can be an organic binder; specifically, the binder is selected from at least one of methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose; the lubricant can be an aliphatic hydrocarbon lubricant, such as paraffin, metal stearate; specifically, the lubricant is sodium stearate.

[0046] In some optional embodiments, the pressure of the extrusion molding in step 1) is 1-30 bar. Most of the glass bubbles do not break during the extrusion molding process, and the single glass bubble maintains a complete spherical shape. Therefore, the pressure of the extrusion molding can be appropriately adjusted according to the compressive strength of the selected glass bubble.

[0047] In some optional embodiments, the first temperature of the first sintering in step 2) is at least 200° C., such as 300° C. to 400° C., and / or the first residence time is at least 1 minute, such as 1 to 10 hours. During the sintering process at this temperature, substances such as solvents and binders in the green body are removed.

[0048] In some optional embodiments, the second temperature of the second sintering is greater than 400°C and less than the softening point of the glass of the glass bubble; for example, 500°C, 600°C, 700°C, etc., and the second residence time is at least 1 minute, for example, 1 to 10 hours. The second temperature is higher than 400°C and lower than the softening point of the glass in the glass bubble. The purpose is to keep the original shape of the blank unchanged. At the same time, since the temperature is already higher than 400°C, the glass component in the glass bubble begins to undergo a phase change, and the disordered glass phase partially crystallizes into a crystalline phase within this temperature range, and the glass bubble is transformed into a glass ceramic bubble. At the same time, due to this transformation, some glass bubbles begin to break and have at least one opening. Therefore, the sintering time within this temperature range can be appropriately adjusted to adjust the crystallinity of the porous glass ceramic. It can be understood that the raw glass bubble itself can also contain a certain proportion of crystalline phases, which can shorten the sintering time in this process.

[0049] In some optional embodiments, the third temperature of the third sintering is greater than the softening point of the glass. Specifically, the softening point temperature of the glass is less than 900°C. The third residence time can be at least 1 minute, for example 1 to 10 hours. At this temperature, the glass component has fluidity, so the adjacent glass-ceramic bubbles are directly bonded to each other. At the same time, since the glass-ceramic bubbles still have a crystalline phase component, the crystalline phase component serves as a skeleton so that its morphology does not collapse and still maintains a basically complete form. In addition, the glass-ceramic bubbles further crack to form a large number of openings, which are interconnected to form pores, and the pores extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

[0050] The third temperature is higher than the softening point of the glass of the glass bubble. The glass ceramic bubble is heated to at least the softening temperature of the amorphous glass, so that most of the glass ceramic bubbles are opened due to the expansion of the gas in the bubble, and the adjacent glass ceramic bubbles are sintered together by heating to form a bond. From the overall point of view, the bonded open glass ceramic bubbles form pores in the porous glass ceramic matrix, which can be used in atomizers and electronic atomization devices to effectively improve the atomization efficiency and liquid guiding effect.

[0051] In some optional embodiments, the mass ratio of glass bubbles to binder, lubricant and water is (80-140): (10-40): (2.5-3.6): (50-85).

[0052] In some optional embodiments, in step 3), the raw material of the heating element may be at least one of electronic paste (metal paste), heating wire or heating mesh. The electronic paste may be directly applied to the surface of the porous glass-ceramic substrate in a preset shape by silk-screen printing, and sintered at a preset temperature. The sintering temperature may be adaptively adjusted according to the type of the binder phase and the metal component in the electronic paste, and the sintering temperature is usually 400-800°C.

[0053] In some optional embodiments, the glass component in the glass bubble may be soda-lime silicate glass, borosilicate glass or other glass. Specifically, the glass component may include: SiO2 74-85%, CaO 6.5-10%, B2O3 5-9%, Al2O3 0.4-2%, Fe2O3 0.01-1%, Na2O 1-3%, K2O 0.1-0.5%.

[0054] In some optional embodiments, step 1) further comprises adding a pore former. Optionally, the pore former is selected from at least one of starch, polymethyl methacrylate (PMMA), polystyrene (PS), and graphite. Optionally, the particle size range of the pore former can be 1-150um. It can be understood that the addition of the pore former can further improve the porosity of the porous glass ceramic matrix while ensuring the strength of the raw glass bubble.

[0055] In some optional embodiments, step 1) further includes a second inorganic material. The second inorganic material may be at least one of clay, talc, silica, and alumina. The melting point or softening point of the above materials is higher than the softening point of the glass in the glass bubble.

[0056] In some optional embodiments, the mass ratio of glass bubbles to binder, slip agent, water, pore former, and second inorganic material is (80-140): (10-40): (2.5-3.6): (50-85): (0-45): (0-7).

[0057] like Figure 5 As shown, the present invention also provides an atomizer, wherein the atomizer includes the atomizer core described above. The atomizer includes a shell, and a liquid storage tank and an atomization cavity are formed in the shell. The liquid storage tank is used to store liquid atomization medium, and the atomization cavity is used to accommodate the atomization core described above. The atomization core can atomize the liquid atomization medium.

[0058] like Figure 6 As shown, the present invention also provides an electronic atomization device, which includes the above-mentioned atomizer 1 and a battery assembly 2. The battery assembly and the atomizer can be an integrated structure or a detachable structure. The battery assembly is used to power the atomizer according to a preset mode, so that the atomizer atomizes the liquid atomization medium according to the preset mode.

[0059] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed by the present invention.

[0060] The glass bubbles of the present invention are made of soda-lime silicate glass. The raw glass bubbles of the same composition are used in the following embodiments, and their D10 is 18.61 μm, D50 is 39.38 μm, D90 is 69.47 μm, and the porosity of the glass bubble monomer is 84.8%. The main components of the raw glass bubbles are Si: 41.647 wt%, O: 49.375 wt%, Na: 3.778 wt%, Ca: 4.619 wt%, Mg: 0.201 wt%, and Al: 0.379 wt%.

[0061] Example 1

[0062] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0063] 1) 80 g of glass bubbles were mixed with 30 g of hydroxyethyl cellulose, 2.5 g of sodium stearate and 80 g of water and extruded to obtain a green body at a molding pressure of 7 bar;

[0064] 2) subjecting the green body in step 1) to first sintering, second sintering and third sintering to obtain a porous glass ceramic matrix, wherein the first sintering temperature is 310° C., the first sintering time is 3 h, the second sintering temperature is 540° C., the second sintering time is 3 h, the third sintering temperature is 1000° C., and the third sintering time is 4 h;

[0065] 3) Printing 310 stainless steel slurry on the porous glass ceramic substrate in step 2), sintering to form, the sintering temperature is 700° C., and the sintering time is 3 hours to obtain the atomizing core.

[0066] Example 2

[0067] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0068] 1) 140 g of glass bubbles were mixed with 35.02 g of hydroxyethyl cellulose, 3.52 g of sodium stearate, 2.78 g of clay and 80.04 g of water and extruded to obtain a green body at a molding pressure of 24 bar;

[0069] 2) subjecting the green body in step 1) to first sintering, second sintering and third sintering to obtain a porous glass-ceramic matrix, wherein the first sintering temperature is 350° C., the first sintering time is 2.5 h, the second sintering temperature is 690° C., the second sintering time is 3 h, the third sintering temperature is 1500° C., and the third sintering time is 3.5 h;

[0070] 3) Printing 310 stainless steel slurry on the porous glass ceramic substrate in step 2), sintering and forming, the sintering temperature is 800° C., and the sintering time is 5 hours to obtain the atomizing core.

[0071] Example 3

[0072] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0073] 1) 135 g of glass bubbles, 40 g of hydroxyethyl cellulose, 3 g of sodium stearate, 7 g of clay and 85 g of water were mixed and extruded to obtain a green body at a molding pressure of 15 bar;

[0074] Step 2) and step 3) are the same as in Example 1, to obtain the atomizer core.

[0075] Comparative Example 1

[0076] This comparative example provides an atomizer core, as described in CN 114668183 A, specifically, the porous body of the atomizer core includes a stacked large-pore structure layer and a small-pore structure layer, wherein the average pore size of the large-pore structure layer is in the range of 50-150 μm, and the average pore size of the small-pore structure layer is in the range of 20-100 μm. The average porosity of the porous body is 50%-75%.

[0077] Comparative Example 2

[0078] This comparative example provides an atomizer core, and a preparation method thereof comprises the following steps:

[0079] 1) 80 g of glass powder was mixed with 30 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 80 g of a pore former and 160 g of water, and the mixture was extruded to obtain a green body at a molding pressure of 20 bar; wherein the pore former was polymethyl methacrylate (PMMA).

[0080] Step 2) and step 3) are the same as in Example 1, to obtain the atomizer core.

[0081] Test Example 1

[0082] The porous matrix in the atomizer core of the embodiment of the present invention and the comparative example was tested for tortuosity, average oil conduction time, porosity, and average pore size. Average oil conduction time test method: the porous matrix of the atomizer core was placed in an oven at 120°C for 15 minutes, and then placed in a drying dish to cool naturally (about 15 minutes), 0.70±0.01g of e-liquid was taken in a metal container dedicated to oil conduction, and the porous matrix was placed in the metal container, and a stopwatch was used to record the time required for the porous matrix to be completely infiltrated by the e-liquid; the test method for porosity, average pore size, and tortuosity was the mercury intrusion method (the test equipment was a mercury intrusion instrument).

[0083] The atomizer core of the embodiment is used to conduct a puffing experiment, and the soot, lifespan, and puffing taste of the electronic atomization device are tested respectively; after a preset number of puffs (the preset number of puffs of the present invention is 500 puffs), the soot on the surface of the atomizer core is observed to determine the deposition of the soot. During the preset number of puffs, it is tested whether there is any failure in this process, and the lifespan is statistically recorded, where the failure situations mainly include: 1. The resistance value of the atomizer core changes significantly abnormally (such as: the resistance value increases significantly due to the breakage and shedding of the heating element); 2. The amount of mist output is less than half of the initial atomization amount. The puffing taste is determined by the tester during the preset 500 puffs to determine whether there is an abnormal taste such as a burnt smell. The above test conditions are 6.5W power, bare chip (not assembled as an atomizer); during the taste test, the atomizer core is assembled as an atomizer for testing.

[0084] Table 1

[0085]

[0086] Test Example 2

[0087] The smoke volume of the atomizer core bare chips of Example 2 and Comparative Example 1 was tested at different powers, and the smoke oils used were strawberry watermelon smoke oil and lake watermelon smoke oil. The specific test method was: the atomizer core was subjected to a smoking experiment, and each smoking process (i.e., each puff) included: smoking for 3s and then pausing for 8s. The smoke volume of each smoking process was tested, and the average value was obtained by statistics.

[0088] The test results are as follows Figure 1 As shown, the atomizer core of Example 2 has a linear increase in smoke volume in the power range of 4.5-6.5W, and a slowing trend at 6.5W. Therefore, the atomizer core has a high atomization efficiency. When tested with Lake Watermelon E-liquid, the atomization efficiency corresponding to 4.5W is 1.51mg / W; the atomization efficiency corresponding to 5.5W is 1.62mg / W; and the atomization efficiency corresponding to 6.5W is 1.56mg / W.

[0089] The atomizer core of comparative example 1: in the range of 4.5-8.5W, the smoke volume increases linearly, and in the range of 4.5-6.5W, the smoke volume is lower than that of the atomizer core of the embodiment.

[0090] The inventors analyzed that: the smaller the tortuosity, the shorter the relative distance of the e-liquid through the atomizer core. Under the same capillary force and other factors, the overall flow time of the atomizer medium is shorter, the amount of smoke is large, and the oil conduction effect is better. For lower power situations, such as: 4.5-6.5W, the atomizer core of the present invention has sufficient liquid supply and high atomization efficiency; however, for higher power situations, the large-aperture atomizer core has more advantages, but the atomizer core with a larger aperture will cause leakage problems. Therefore, the atomizer core of the present invention has both liquid conduction rate, atomization efficiency and liquid locking effect.

[0091] Test Example 3

[0092] The atomizer core of Example 2 was tested for temperature field distribution, and the test e-liquid was fruit (watermelon) flavored e-liquid. Test method: The atomizer core was assembled with an atomizer and an electronic atomization device, and a puffing experiment was performed. Each puffing process (i.e., each puff) included: puffing for 3 seconds and then pausing for 8 seconds. The temperature field of the atomizer core was measured using an infrared thermometer to obtain the distribution of the temperature field, and then the distribution statistics of the temperature field were performed; a total of 5 parallel samples were tested, which were recorded as samples 1 to 5.

[0093] The test results are further shown in Figure 2 and Figure 3 shown. Figure 2 The horizontal axis is time, in seconds (s), which means the total number of puffs is 20. Figure 2 The vertical axis is temperature, in degrees Celsius (℃); Figure 2 As shown, during each puff (each puff), the temperature of the main atomization zone is between 250-300°C; Figure 3 The figure shows the temperature field distribution diagram of one of the samples (sample 1) in one mouth. There is no individual high temperature area (area exceeding 310°C), which shows that the overall liquid supply of the atomizer core is sufficient and the porous matrix has a good liquid conduction effect. Figure 4 As shown, the scale accumulation on the atomizing surface of the sample after 300 mouth tests. Although there is a small amount of scale, the scale is relatively evenly distributed in the entire atomizing surface area and does not gather on the surface of the heating element. Therefore, it is beneficial to improve the overall service life.

[0094] Therefore, the inventors analyzed and believed that: the temperature field is concentrated in the high-efficiency area, and there is a certain temperature field gradient; therefore, the atomization efficiency is high, scaling is not easy, and at the same time, it has a rich taste level.

[0095] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. An atomizing core, It is characterized in that The atomizing core comprises a porous substrate and a heating element. The porous substrate is a porous glass ceramic substrate. The tortuosity of the porous glass ceramic substrate is 1-2.

5.

2. The atomizer core according to claim 1, It is characterized in that The tortuosity of the porous glass-ceramic substrate is 1-2.

3. The atomizer core according to claim 2, It is characterized in that The tortuosity of the porous glass-ceramic substrate is 1.3-1.

9.

4. The atomizer core according to any one of claims 1 to 3, It is characterized in that The porosity of the porous glass-ceramic matrix is ​​greater than 50%; Optionally, the porosity of the porous glass-ceramic matrix is ​​60-80%.

5. The atomizer core according to any one of claims 1 to 4, It is characterized in that The average pore size of the porous glass-ceramic matrix is ​​15-45 μm.

6. The atomizer core according to any one of claims 1 to 5, It is characterized in that The porous glass-ceramic matrix includes pores formed by openings of glass-ceramic bubbles.

7. The atomizer core according to any one of claims 1 to 6, It is characterized in that The heating element is a metal heating film; The heating element is arranged on at least one surface of the porous glass-ceramic substrate.

8. The atomizer core according to claim 7, It is characterized in that The metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

9. An atomizer, It is characterized in that The atomizer comprises the atomizer core according to any one of claims 1 to 8.

10. An electronic atomization device, It is characterized in that The electronic atomization device includes the atomizer according to claim 9 and also includes a battery assembly.

Citation Information

Cited By

  • Atomization core, atomizer, and electronic atomization device

    EP4721591A1