Injection molding production process and injection mold for automotive upholstery

By pretreating molds and adding mold release agents and alloy elements in the automotive injection molding process, unevenly brushing and bubble problems in the prior art are solved, and the quality and mechanical properties of injection molded parts are improved.

CN119058006APending Publication Date: 2024-12-03NANCHANGXING ELECTRONIC CONTROL SYST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411354584.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the injection molding process of existing automobile injection molding parts, the release agent is not brushed uniformly enough, and it is easy to brush too much. In addition, bubbles are easily generated inside the injection molding parts, and the raw materials are not tightly combined, resulting in poor mechanical performance and low pass rate.

Method used

Adopt an injection molding production process for automotive interior parts, including mold pretreatment, uniform brushing of mold release agent, preheating of mold, heating and melting of injection molding raw materials and stirring evenly. Through multiple injection molding and vibrating the mold, combining water-cooled cooling and high-pressure gas Demolding to ensure that the raw materials are closely combined, and alloy elements such as Ni, Mo, V are added to the injection mold to improve material strength and wear resistance.

Benefits of technology

The mold release agent is uniformly applied, the bubbles inside the injection molded parts are removed, the density of raw materials is improved, the quality and mechanical properties of the injection molded parts are significantly improved, and the service life is extended.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an injection molding production process and an injection mold for automotive upholstery, and the injection molding production process comprises the following steps: mold pretreatment: preparing the injection mold, cleaning the injection mold, and drying the injection mold after cleaning; brushing a release agent: selecting the release agent, and uniformly brushing the release agent on the inner surface of the injection mold dried in the step S1; preheating an injection mold; processing injection molding raw materials; the prepared injection molding solution is injected into a mold through an injection molding nozzle, injection molding is divided into multiple times, injection molding is stopped for 3-5 seconds after each time of injection molding, and the mold is vibrated through a vibration machine till multiple times of injection molding are completed; cooling the mold; opening the mold and demolding; and treating the interior trim parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of injection molding technology, and in particular relates to an injection molding production process and an injection molding mold for automobile interior decoration parts. Background Art

[0002] Nowadays, the injection molding process is developing towards shortening the injection molding cycle and improving production efficiency. Generally, in order to improve production efficiency, the injection molding process of the injection mold adopts the methods of increasing plasticizing capacity, shortening injection time, and accelerating template movement speed. In addition, the improvement of the injection method of the injection mold, the improvement of the mold closing method, the change of cooling efficiency method, etc. are also adopted. The purpose is to save time, shorten the production cycle and increase output.

[0003] For example, a Chinese patent with application publication number CN107571448A discloses an injection molding production process for automobile injection molding parts. The raw materials of automobile injection molding parts are polypropylene and polyethylene, and the polypropylene and polyethylene are dried in an oven. Then, the mold of the automobile injection molding parts is preheated, and the molten polypropylene is injected into the preheated mold through a nozzle. After the mold is closed, the pressure is maintained, and circulating water is used for cooling. After demolding, the surface is treated to obtain automobile injection molding parts. The present invention enables automobile injection molding parts to use the above process to improve production efficiency, reduce production costs, and improve the quality of finished products. Automobile injection molding parts have high overall rigidity, long service life, and improved safety performance; an ozonated layer is formed on the surface of the injection molding part, which can assume the function of a protective layer and prevent ozone from further invading the injection molding part, has good wear resistance, and extends its service life.

[0004] However, in the existing automobile injection molding process, the mold release agent is not applied evenly during operation, and it is easy to apply too much mold release agent. In addition, bubbles are easily generated inside the obtained injection molded parts, the raw materials are not tightly combined, the mechanical properties are poor, and the qualified rate is relatively low. Summary of the invention

[0005] Purpose of the invention: In view of the deficiencies in the prior art, the present invention proposes an injection molding production process and an injection mold for automotive interior trim parts.

[0006] Technical solution: The injection molding production process of an automobile interior decoration part described in the present invention comprises the following steps:

[0007] (1) Mold pretreatment: prepare the injection mold, clean the injection mold, and dry it after cleaning;

[0008] (2) Applying a mold release agent: Selecting a mold release agent and applying the mold release agent evenly to the inner surface of the injection mold after the drying treatment in step S1;

[0009] (3) Preheating the injection mold: close the mold and preheat the injection mold;

[0010] (4) Injection molding raw material processing: Select the injection molding raw material, heat and melt the injection molding raw material and stir it evenly to make an injection molding melt for standby use;

[0011] (5) Mold injection molding: The prepared injection molding solution is injected into the mold through the injection nozzle, and the injection molding is divided into multiple injection moldings. After each injection molding, stop for 3-5 seconds and vibrate the mold through a vibration machine until the multiple injection moldings are completed;

[0012] (6) Mold cooling: Use cooling water to spray the surface of the mold and cool the mold with water. The temperature of the cooling water is 20-30°C until the mold and the internal melt are completely cooled to room temperature;

[0013] (7) Mold opening and demolding: the cooled mold is opened, and high-pressure gas is injected into the mold through the injection nozzle to demold the mold, thereby obtaining an injection molded blank;

[0014] (8) Interior decoration processing: The injection molding interface and burr position of the injection molded blank are cut and polished to obtain the interior decoration parts.

[0015] In some embodiments, the release agent is selected from one of silicone methyl branched silicone oil, polyethylene wax, fluororesin powder, and mica powder.

[0016] In some embodiments, the preheating temperature of the injection mold is 150-200° C., and the preheating time is 10-20 minutes.

[0017] In some embodiments, a heat stabilizer, a flame retardant and a modifier are added to the injection molding raw material, and during mixing and stirring, a high-speed stirrer is used for mixing and stirring, the stirring speed is 100 r / min, the stirring time is 10-15 minutes, and the heating temperature during stirring is 100-120°C.

[0018] In some embodiments, the vibration machine is an ultrasonic vibration machine, and the ultrasonic vibration machine works for 3-5 seconds each time.

[0019] In some embodiments, after the injection molding in step (5) is completed, the mold needs to be subjected to pressure-maintaining treatment, and pressure needs to be continuously applied to the inside of the mold. The applied pressure value is 50-70kg / cm3, and the pressure-maintaining time is 40-60 minutes.

[0020] In some embodiments, the material composition of the injection mold includes the following components in mass percentage:

[0021] C: 0.30~0.40%; Si: 0.20~0.40%; Mn: 1.2~1.5%; Cr: 1.5~2.0%; Mo: 1.5~2.0%; Ni: 0.8~1.2%; V: 0.2~0.4%, and the balance is Fe.

[0022] In some embodiments, the Si is added in the form of ferrosilicon containing 73% Si, the Mn is added in the form of ferromanganese containing 65% Mn, the Cr is added in the form of low-carbon ferrochrome containing 57% Cr, the Mo is added in the form of molybdenum plate containing 55% Mo, the Ni is added in the form of pure nickel plate, and the V is added in the form of ferrovanadium containing 50% V.

[0023] Beneficial effects: The beneficial effects of the present invention are as follows:

[0024] (1) The injection molding process of the present invention can evenly and fully apply the mold release agent to the inside of the mold, remove excess mold release agent, and fully remove bubbles formed when the raw materials are injected, so that the raw materials inside the mold are tightly and firmly combined, greatly improving the quality of the injection molded parts;

[0025] (2) The injection mold used in the present invention adds alloy elements such as Ni, Mo, and V to medium carbon steel during the formulation process, which refines the grains, improves hardenability, and improves the strength, wear resistance, and plastic toughness of the material. Ni and Cr alloy elements are also beneficial to improving the corrosion resistance of the injection mold;

[0026] (3) The injection mold used in the present invention uses vacuum induction sintering as the mold material, the molten metal is free of oxidation, the smelted metal is of high purity, and the metallurgical quality of the material is effectively improved, thereby improving the comprehensive performance of the material;

[0027] (4) The injection mold used in the present invention is quenched in a vacuum quenching furnace, and the mold material is heated evenly to prevent oxidation and decarburization of the material, so as to ensure the carbon content in the martensite of the mold steel after quenching and ensure a high hardness;

[0028] (5) The injection mold used in the present invention uses cryogenic treatment on the mold steel in a freezer, which promotes the further transformation of the retained austenite into martensite, stabilizes the structure, and thus ensures the dimensional stability. This process is easier to implement than the previous nitrogen cryogenic treatment and has a lower cost;

[0029] (6) The injection mold used in the present invention has its concave and convex mold surfaces laser quenched. This process ensures that the mold core has good toughness while also improving the hardness of the working surface, thereby increasing the service life of the mold. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific embodiments:

[0031] Example 1

[0032] An injection molding production process for automobile interior decoration parts comprises the following steps:

[0033] (1) Mold pretreatment: prepare the injection mold, clean the injection mold, and dry it after cleaning;

[0034] (2) applying a mold release agent: selecting a mold release agent and applying the mold release agent evenly to the inner surface of the injection mold after the drying treatment in step S1, wherein the mold release agent is selected from silicone resin methyl branched silicone oil;

[0035] (3) Preheating the injection mold: close the mold and preheat the injection mold at a temperature of 150°C for 10 minutes;

[0036] (4) Injection molding raw material processing: selecting injection molding raw materials, heating and melting the injection molding raw materials and stirring them evenly to prepare injection molding melt for standby use; heat stabilizer, flame retardant and modifier are added to the injection molding raw materials, and during mixing and stirring, a high-speed stirrer is used for mixing and stirring, the stirring speed is 100 r / min, the stirring time is 10 minutes, and the heating temperature during stirring is 100° C.;

[0037] (5) Mold injection molding: The prepared injection molding solution is injected into the mold through the injection molding nozzle, and the injection molding is divided into multiple injection moldings. After each injection molding, stop for 3-5 seconds, and vibrate the mold through a vibration machine until multiple injection moldings are completed; the vibration machine uses an ultrasonic vibration machine, and the ultrasonic vibration machine works for 3 seconds each time; after the injection molding is completed, the mold needs to be pressure-maintained, and the pressure applied inside the mold needs to be continuously applied. The pressure value is 50kg / cm3, and the pressure holding time is 40 minutes;

[0038] (6) Mold cooling: Use cooling water to spray the surface of the mold and cool the mold with water. The temperature of the cooling water is 20-30°C until the mold and the internal melt are completely cooled to room temperature;

[0039] (7) Mold opening and demolding: the cooled mold is opened, and high-pressure gas is injected into the mold through the injection nozzle to demold the mold, thereby obtaining an injection molded blank;

[0040] (8) Interior decoration processing: The injection molding interface and burr position of the injection molded blank are cut and polished to obtain the interior decoration parts.

[0041] In this embodiment, the material composition of the injection mold includes the following components in mass percentage:

[0042] C: 0.30%; Si: 0.20%; Mn: 1.2%; Cr: 1.5%; Mo: 1.5%; Ni: 0.8%; V: 0.2%, and the balance is Fe.

[0043] Among them, the Si is added in the form of ferrosilicon containing 73% Si, the Mn is added in the form of ferromanganese containing 65% Mn, the Cr is added in the form of low-carbon ferrochrome containing 57% Cr, the Mo is added in the form of molybdenum plate containing 55% Mo, the Ni is added in the form of pure nickel plate, and the V is added in the form of ferrovanadium with 50% V.

[0044] Among them, C makes the material have better comprehensive mechanical properties (strength and toughness) after heat treatment; Si has a solid solution strengthening effect and improves hardenability; Mn can prevent hot brittleness and strongly improve the hardenability of steel to improve wear resistance; Cr can increase the high-temperature oxidation resistance and corrosion resistance of oxidizing media of steel; Mo improves hardenability, reduces or inhibits the tempering brittleness of other alloying elements, and improves thermal strength; Ni has the effect of refining grains, improving the plasticity and toughness of steel, and improving the corrosion resistance of steel; V can improve the tempering resistance of steel, has a strong secondary hardening effect, and has the effect of oxidizing grains.

[0045] The method for preparing the above-mentioned high-performance injection mold material comprises the following steps:

[0046] S1. According to the mass ratio of each element, select suitable raw materials for calculation and batching;

[0047] S2, put the prepared raw materials into the crucible of the vacuum induction melting furnace, cover the furnace cover, close the vent valve, start the vacuum pump to evacuate, adjust the vacuum degree to 5Pa, heat the melting furnace, melt at a high temperature, and refine at a temperature of 1500°C; finally, stop heating after completion, and take out the mold ingot after solidification for 30 minutes;

[0048] S3. Cut off the pouring and riser, then clean the surface of the ingot, calculate the blanking length according to the blanking weight, and cut and blank:

[0049] S4. According to the size requirements of the injection mold, the ingot is forged and stretched into a rod;

[0050] S5, heating the rod material to 840°C in a vacuum water quenching furnace and keeping the temperature for 40 minutes, wherein the vacuum degree of the vacuum water quenching furnace is not higher than 50Pa, and then rapidly quenching and cooling to room temperature by water;

[0051] S6, placing the rod material after quenching treatment in S5 into a freezer for cold treatment at a temperature range of -80°C, further reducing the amount of retained austenite and promoting the transformation of martensite structure;

[0052] S7, tempering the deep-cold treated rod material at 600-650°C to obtain a tempered troostite structure with excellent comprehensive performance, and the troostite hardness is 30-35HRC;

[0053] S8, the rod material treated in S7 is straightened and machined, and the surface of the concave and convex molds after machining is subjected to laser quenching heat treatment, and the thickness of the hardened layer of the laser quenching heat treatment is 0.15mm and the hardness is 58-62HRC;

[0054] S9, assembling the concave and convex molds and other components processed by S8 to obtain a high-performance injection mold.

[0055] Example 2

[0056] An injection molding production process for automobile interior decoration parts comprises the following steps:

[0057] (1) Mold pretreatment: prepare the injection mold, clean the injection mold, and dry it after cleaning;

[0058] (2) applying a mold release agent: selecting a mold release agent and applying the mold release agent evenly to the inner surface of the injection mold after the drying treatment in step S1, wherein the mold release agent is polyethylene wax;

[0059] (3) Preheating the injection mold: close the mold and preheat the injection mold at a temperature of 160°C for 12 minutes;

[0060] (4) Injection molding raw material processing: selecting injection molding raw materials, heating and melting the injection molding raw materials and stirring them evenly to prepare injection molding melt for standby use; heat stabilizer, flame retardant and modifier are added to the injection molding raw materials, and during mixing and stirring, a high-speed stirrer is used for mixing and stirring, the stirring speed is 100 r / min, the stirring time is 12 minutes, and the heating temperature during stirring is 105°C;

[0061] (5) Mold injection molding: The prepared injection molding solution is injected into the mold through the injection molding nozzle, and the injection molding is divided into multiple injection moldings. After each injection molding, stop for 3-5 seconds, and vibrate the mold through a vibration machine until multiple injection moldings are completed; the vibration machine uses an ultrasonic vibration machine, and the ultrasonic vibration machine works for 3 seconds each time; after the injection molding is completed, the mold needs to be pressure-maintained, and the pressure applied inside the mold needs to be continuously applied. The pressure value is 55kg / cm3, and the pressure holding time is 45 minutes;

[0062] (6) Mold cooling: Use cooling water to spray the surface of the mold and cool the mold with water. The temperature of the cooling water is 20-30°C until the mold and the internal melt are completely cooled to room temperature;

[0063] (7) Mold opening and demolding: the cooled mold is opened, and high-pressure gas is injected into the mold through the injection nozzle to demold the mold, thereby obtaining an injection molded blank;

[0064] (8) Interior decoration processing: The injection molding interface and burr position of the injection molded blank are cut and polished to obtain the interior decoration parts.

[0065] In this embodiment, the material composition of the injection mold includes the following components in mass percentage:

[0066] C: 0.32%; Si: 0.22%; Mn: 1.3%; Cr: 1.6%; Mo: 1.6%; Ni: 0.9%; V: 0.25%, and the balance is Fe.

[0067] Among them, the Si is added in the form of ferrosilicon containing 73% Si, the Mn is added in the form of ferromanganese containing 65% Mn, the Cr is added in the form of low-carbon ferrochrome containing 57% Cr, the Mo is added in the form of molybdenum plate containing 55% Mo, the Ni is added in the form of pure nickel plate, and the V is added in the form of ferrovanadium with 50% V.

[0068] Among them, C makes the material have better comprehensive mechanical properties (strength and toughness) after heat treatment; Si has a solid solution strengthening effect and improves hardenability; Mn can prevent hot brittleness and strongly improve the hardenability of steel to improve wear resistance; Cr can increase the high-temperature oxidation resistance and corrosion resistance of oxidizing media of steel; Mo improves hardenability, reduces or inhibits the tempering brittleness of other alloying elements, and improves thermal strength; Ni has the effect of refining grains, improving the plasticity and toughness of steel, and can improve the corrosion resistance of steel; V can improve the tempering resistance of steel, has a strong secondary hardening effect, and has the effect of oxidizing grains.

[0069] The method for preparing the above-mentioned high-performance injection mold material comprises the following steps:

[0070] S1. According to the mass ratio of each element, select suitable raw materials for calculation and batching;

[0071] S2. Put the prepared raw materials into the crucible of the vacuum induction melting furnace, cover the furnace cover, close the vent valve, start the vacuum pump to evacuate, adjust the vacuum degree to 10Pa, heat the melting furnace, melt at high temperature, and refine at a temperature of 1510°C; finally, stop heating after completion, and take out the mold ingot after solidification for 35 minutes;

[0072] S3. Cut off the pouring and riser, then clean the surface of the ingot, calculate the blanking length according to the blanking weight, and cut and blank:

[0073] S4. According to the size requirements of the injection mold, the ingot is forged and stretched into a rod;

[0074] S5, heating the rod material to 845°C in a vacuum water quenching furnace and keeping the temperature for 45 minutes, wherein the vacuum degree of the vacuum water quenching furnace is not higher than 50Pa, and then rapidly quenching and cooling the rod material to room temperature by water;

[0075] S6, placing the rod material after quenching treatment in S5 into a freezer for cold treatment at a temperature range of -75°C, further reducing the amount of retained austenite and promoting the transformation of martensite structure;

[0076] S7, tempering the deep-cold treated rod material at 610°C to obtain a tempered troostite structure with excellent comprehensive performance, and the troostite hardness is 30-35HRC;

[0077] S8, the rod material treated in S7 is straightened and machined, and the surface of the concave and convex molds after machining is subjected to laser quenching heat treatment, and the thickness of the hardened layer of the laser quenching heat treatment is 0.20mm and the hardness is 58-62HRC;

[0078] S9, assembling the concave and convex molds and other components processed by S8 to obtain a high-performance injection mold.

[0079] Example 3

[0080] An injection molding production process for automobile interior decoration parts comprises the following steps:

[0081] (1) Mold pretreatment: prepare the injection mold, clean the injection mold, and dry it after cleaning;

[0082] (2) Applying a mold release agent: Select a mold release agent and apply the mold release agent evenly to the inner surface of the injection mold after the drying treatment in step S1. The mold release agent is fluororesin powder;

[0083] (3) Preheating the injection mold: close the mold and preheat the injection mold at a temperature of 170°C for 15 minutes;

[0084] (4) Injection molding raw material processing: selecting injection molding raw materials, heating and melting the injection molding raw materials and stirring them evenly to prepare injection molding melt for standby use; heat stabilizer, flame retardant and modifier are added to the injection molding raw materials, and during mixing and stirring, a high-speed stirrer is used for mixing and stirring, the stirring speed is 100 r / min, the stirring time is 13 minutes, and the heating temperature during stirring is 110°C;

[0085] (5) Mold injection molding: The prepared injection molding solution is injected into the mold through the injection molding nozzle, and the injection molding is divided into multiple injection moldings. After each injection molding, stop for 3-5 seconds, and vibrate the mold through a vibration machine until multiple injection moldings are completed; the vibration machine uses an ultrasonic vibration machine, and the ultrasonic vibration machine works for 4 seconds each time; after the injection molding is completed, the mold needs to be pressure-maintained, and the pressure applied inside the mold needs to be continuously applied. The pressure value is 60kg / cm3, and the pressure holding time is 50 minutes;

[0086] (6) Mold cooling: Use cooling water to spray the surface of the mold and cool the mold with water. The temperature of the cooling water is 20-30°C until the mold and the internal melt are completely cooled to room temperature;

[0087] (7) Mold opening and demolding: the cooled mold is opened, and high-pressure gas is injected into the mold through the injection nozzle to demold the mold, thereby obtaining an injection molded blank;

[0088] (8) Interior decoration processing: The injection molding interface and burr position of the injection molded blank are cut and polished to obtain the interior decoration parts.

[0089] In this embodiment, the material composition of the injection mold includes the following components in mass percentage:

[0090] C: 0.30%, Si: 0.40%, Mn: 1.5%, Cr: 1.8%, Mo: 1.5%, Ni: 1.0%, V: 0.2%, and the balance is Fe.

[0091] Among them, the Si is added in the form of ferrosilicon containing 73% Si, the Mn is added in the form of ferromanganese containing 65% Mn, the Cr is added in the form of low-carbon ferrochrome containing 57% Cr, the Mo is added in the form of molybdenum plate containing 55% Mo, the Ni is added in the form of pure nickel plate, and the V is added in the form of ferrovanadium with 50% V.

[0092] Among them, C makes the material have better comprehensive mechanical properties (strength and toughness) after heat treatment; Si has a solid solution strengthening effect and improves hardenability; Mn can prevent hot brittleness and strongly improve the hardenability of steel to improve wear resistance; Cr can increase the high-temperature oxidation resistance and corrosion resistance of oxidizing media of steel; Mo improves hardenability, reduces or inhibits the tempering brittleness of other alloying elements, and improves thermal strength; Ni has the effect of refining grains, improving the plasticity and toughness of steel, and improving the corrosion resistance of steel; V can improve the tempering resistance of steel, has a strong secondary hardening effect, and has the effect of oxidizing grains.

[0093] The method for preparing the above-mentioned high-performance injection mold material comprises the following steps:

[0094] S1. According to the mass ratio of each element, select suitable raw materials for calculation and batching;

[0095] S2, put the prepared raw materials into the crucible of the vacuum induction melting furnace, cover the furnace cover, close the vent valve, start the vacuum pump to evacuate, adjust the vacuum degree to 15Pa, heat the melting furnace, melt at a high temperature, and refine at a temperature of 1520°C; finally, stop heating after completion, and take out the mold ingot after solidification for 35 minutes;

[0096] S3. Cut off the pouring and riser, then clean the surface of the ingot, calculate the blanking length according to the blanking weight, and cut and blank:

[0097] S4. According to the size requirements of the injection mold, the ingot is forged and stretched into a rod;

[0098] S5, heating the rod material to 850°C in a vacuum water quenching furnace for 50 minutes, wherein the vacuum degree of the vacuum water quenching furnace is not higher than 50Pa, and then rapidly quenching and cooling to room temperature by water;

[0099] S6, placing the rod material after quenching treatment in S5 into a freezer for cold treatment at a temperature range of -75°C, further reducing the amount of retained austenite and promoting the transformation of martensite structure;

[0100] S7, tempering the deep-cold treated rod material at 620°C to obtain a tempered troostite structure with excellent comprehensive performance, and the troostite hardness is 30-35HRC;

[0101] S8, the rod material treated in S7 is straightened and machined, and the surface of the concave and convex molds after machining is subjected to laser quenching heat treatment, and the thickness of the hardened layer of the laser quenching heat treatment is 0.20mm and the hardness is 58-62HRC;

[0102] S9, assembling the concave and convex molds and other components processed by S8 to obtain a high-performance injection mold.

[0103] Example 4

[0104] An injection molding production process for automobile interior decoration parts comprises the following steps:

[0105] (1) Mold pretreatment: prepare the injection mold, clean the injection mold, and dry it after cleaning;

[0106] (2) applying a mold release agent: selecting a mold release agent and evenly applying the mold release agent to the inner surface of the injection mold after the drying treatment in step S1, wherein the mold release agent is mica powder;

[0107] (3) Preheating the injection mold: close the mold and preheat the injection mold at a temperature of 180°C for 16 minutes;

[0108] (4) Injection molding raw material processing: selecting injection molding raw materials, heating and melting the injection molding raw materials and stirring them evenly to prepare injection molding melt for standby use; heat stabilizer, flame retardant and modifier are added to the injection molding raw materials, and during mixing and stirring, a high-speed stirrer is used for mixing and stirring, the stirring speed is 100 r / min, the stirring time is 13 minutes, and the heating temperature during stirring is 115°C;

[0109] (5) Mold injection molding: The prepared injection molding solution is injected into the mold through the injection nozzle, and the injection molding is divided into multiple injection moldings. After each injection molding, stop for 3-5 seconds, and vibrate the mold through a vibration machine until multiple injection moldings are completed; the vibration machine uses an ultrasonic vibration machine, and the ultrasonic vibration machine works for 5 seconds each time; after the injection molding is completed, the mold needs to be pressure-maintained, and the pressure applied inside the mold needs to be continuously applied. The pressure value is 65kg / cm3, and the pressure holding time is 55 minutes;

[0110] (6) Mold cooling: Use cooling water to spray the surface of the mold and cool the mold with water. The temperature of the cooling water is 20-30°C until the mold and the internal melt are completely cooled to room temperature;

[0111] (7) Mold opening and demolding: the cooled mold is opened, and high-pressure gas is injected into the mold through the injection nozzle to demold the mold, thereby obtaining an injection molded blank;

[0112] (8) Interior decoration processing: The injection molding interface and burr position of the injection molded blank are cut and polished to obtain the interior decoration parts.

[0113] In this embodiment, the material composition of the injection mold includes the following components in mass percentage:

[0114] C: 0.38%; Si: 0.32%; Mn: 1.4%; Cr: 1.8%; Mo: 1.8%; Ni: 1.0%; V: 0.3%, and the balance is Fe.

[0115] Among them, the Si is added in the form of ferrosilicon containing 73% Si, the Mn is added in the form of ferromanganese containing 65% Mn, the Cr is added in the form of low-carbon ferrochrome containing 57% Cr, the Mo is added in the form of molybdenum plate containing 55% Mo, the Ni is added in the form of pure nickel plate, and the V is added in the form of ferrovanadium with 50% V.

[0116] Among them, C makes the material have better comprehensive mechanical properties (strength and toughness) after heat treatment; Si has a solid solution strengthening effect and improves hardenability; Mn can prevent hot brittleness and strongly improve the hardenability of steel to improve wear resistance; Cr can increase the high-temperature oxidation resistance and corrosion resistance of oxidizing media of steel; Mo improves hardenability, reduces or inhibits the tempering brittleness of other alloying elements, and improves thermal strength; Ni has the effect of refining grains, improving the plasticity and toughness of steel, and improving the corrosion resistance of steel; V can improve the tempering resistance of steel, has a strong secondary hardening effect, and has the effect of oxidizing grains.

[0117] The method for preparing the above-mentioned high-performance injection mold material comprises the following steps:

[0118] S1. According to the mass ratio of each element, select suitable raw materials for calculation and batching;

[0119] S2, put the prepared raw materials into the crucible of the vacuum induction melting furnace, cover the furnace cover, close the vent valve, start the vacuum pump to evacuate, adjust the vacuum degree to 18Pa, heat the melting furnace, melt at a high temperature, and refine at a temperature of 1530°C; finally, stop heating after completion, and take out the mold ingot after solidification for 30 minutes;

[0120] S3. Cut off the pouring and riser, then clean the surface of the ingot, calculate the blanking length according to the blanking weight, and cut and blank:

[0121] S4. According to the size requirements of the injection mold, the ingot is forged and stretched into a rod;

[0122] S5, heating the rod material to 850°C in a vacuum water quenching furnace for 60 minutes, wherein the vacuum degree of the vacuum water quenching furnace is not higher than 50Pa, and then rapidly quenching and cooling to room temperature by water;

[0123] S6, placing the rod material after quenching treatment in S5 into a freezer for cold treatment at a temperature range of -75°C, further reducing the amount of retained austenite and promoting the transformation of martensite structure;

[0124] S7, tempering the deep-cold treated rod material at 640°C to obtain a tempered troostite structure with excellent comprehensive performance, and the troostite hardness is 30-35HRC;

[0125] S8, the rod material treated in S7 is straightened and machined, and the surfaces of the concave and convex molds after machining are subjected to laser quenching heat treatment, and the thickness of the hardened layer of the laser quenching heat treatment is 0.25mm and the hardness is 58-62HRC;

[0126] S9, assembling the concave and convex molds and other components processed by S8 to obtain a high-performance injection mold.

[0127] Example 5

[0128] An injection molding production process for automobile interior decoration parts comprises the following steps:

[0129] (1) Mold pretreatment: prepare the injection mold, clean the injection mold, and dry it after cleaning;

[0130] (2) applying a mold release agent: selecting a mold release agent and applying the mold release agent evenly to the inner surface of the injection mold after the drying treatment in step S1, wherein the mold release agent is selected from silicone resin methyl branched silicone oil;

[0131] (3) Preheating the injection mold: close the mold and preheat the injection mold at a temperature of 1200°C for 20 minutes;

[0132] (4) Injection molding raw material processing: Select injection molding raw materials, heat and melt the injection molding raw materials and stir them evenly to make injection molding melt for standby use; heat stabilizer, flame retardant and modifier are added to the injection molding raw materials, and during mixing and stirring, a high-speed stirrer is used for mixing and stirring, the stirring speed is 100r / min, the stirring time is 15 minutes, and the heating temperature during stirring is 120°C;

[0133] (5) Mold injection molding: The prepared injection molding solution is injected into the mold through the injection molding nozzle, and the injection molding is divided into multiple injection moldings. After each injection molding, stop for 3-5 seconds, and vibrate the mold through a vibration machine until multiple injection moldings are completed; the vibration machine uses an ultrasonic vibration machine, and the ultrasonic vibration machine works for 5 seconds each time; after the injection molding is completed, the mold needs to be pressure-maintained, and the pressure applied inside the mold needs to be continuously applied. The pressure value applied is 70kg / cm3, and the pressure holding time is 60 minutes;

[0134] (6) Mold cooling: Use cooling water to spray the surface of the mold and cool the mold with water. The temperature of the cooling water is 20-30°C until the mold and the internal melt are completely cooled to room temperature;

[0135] (7) Mold opening and demolding: the cooled mold is opened, and high-pressure gas is injected into the mold through the injection nozzle to demold the mold, thereby obtaining an injection molded blank;

[0136] (8) Interior decoration processing: The injection molding interface and burr position of the injection molded blank are cut and polished to obtain the interior decoration parts.

[0137] In this embodiment, the material composition of the injection mold includes the following components in mass percentage:

[0138] C: 0.40%; Si: 0.40%; Mn: 1.5%; Cr: 2.0%; Mo: 2.0%; Ni: 1.2%; V: 0.4%, and the balance is Fe.

[0139] Among them, the Si is added in the form of ferrosilicon containing 73% Si, the Mn is added in the form of ferromanganese containing 65% Mn, the Cr is added in the form of low-carbon ferrochrome containing 57% Cr, the Mo is added in the form of molybdenum plate containing 55% Mo, the Ni is added in the form of pure nickel plate, and the V is added in the form of ferrovanadium with 50% V.

[0140] Among them, C makes the material have better comprehensive mechanical properties (strength and toughness) after heat treatment; Si has a solid solution strengthening effect and improves hardenability; Mn can prevent hot brittleness and strongly improve the hardenability of steel to improve wear resistance; Cr can increase the high-temperature oxidation resistance and corrosion resistance of oxidizing media of steel; Mo improves hardenability, reduces or inhibits the tempering brittleness of other alloying elements, and improves thermal strength; Ni has the effect of refining grains, improving the plasticity and toughness of steel, and improving the corrosion resistance of steel; V can improve the tempering resistance of steel, has a strong secondary hardening effect, and has the effect of oxidizing grains.

[0141] The method for preparing the above-mentioned high-performance injection mold material comprises the following steps:

[0142] S1. According to the mass ratio of each element, select suitable raw materials for calculation and batching;

[0143] S2, put the prepared raw materials into the crucible of the vacuum induction melting furnace, cover the furnace cover, close the vent valve, start the vacuum pump to evacuate, adjust the vacuum degree to 20Pa, heat the melting furnace, melt at a high temperature, and refine at a temperature of 1540°C; finally, stop heating after completion, and take out the mold ingot after solidification for 40 minutes;

[0144] S3. Cut off the pouring and riser, then clean the surface of the ingot, calculate the blanking length according to the blanking weight, and cut and blank:

[0145] S4. According to the size requirements of the injection mold, the ingot is forged and stretched into a rod;

[0146] S5, heating the rod material to 860°C in a vacuum water quenching furnace for 80 minutes, wherein the vacuum degree of the vacuum water quenching furnace is not higher than 50Pa, and then rapidly quenching and cooling to room temperature by water;

[0147] S6, placing the rod material after quenching treatment in S5 into a freezer for cold treatment, the cold treatment temperature range is -80 to -70°C, further reducing the amount of retained austenite and promoting the transformation of martensite structure;

[0148] S7, tempering the deep-cold treated rod material at 650°C to obtain a tempered troostite structure with excellent comprehensive performance, and the troostite hardness is 30-35HRC;

[0149] S8, the rod material treated in S7 is straightened and machined, and the surfaces of the concave and convex molds after machining are subjected to laser quenching heat treatment, and the thickness of the hardened layer of the laser quenching heat treatment is 0.30mm and the hardness is 58-62HRC;

[0150] S9, assembling the concave and convex molds and other components processed by S8 to obtain a high-performance injection mold.

[0151] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. An injection molding production process for automobile interior decoration parts, characterized in that: The steps include: (1) Mold pretreatment: prepare the injection mold, clean the injection mold, and dry it after cleaning; (2) Applying a mold release agent: Selecting a mold release agent and applying the mold release agent evenly to the inner surface of the injection mold after the drying treatment in step S1; (3) Preheating the injection mold: close the mold and preheat the injection mold; (4) Injection molding raw material processing: Select the injection molding raw material, heat and melt the injection molding raw material and stir it evenly to make an injection molding melt for standby use; (5) Mold injection molding: The prepared injection molding solution is injected into the mold through the injection nozzle, and the injection molding is divided into multiple injection moldings. After each injection molding, stop for 3-5 seconds and vibrate the mold through a vibration machine until the multiple injection moldings are completed; (6) Mold cooling: Use cooling water to spray the surface of the mold and cool the mold with water. The temperature of the cooling water is 20-30°C until the mold and the internal melt are completely cooled to room temperature; (7) Mold opening and demolding: the cooled mold is opened, and high-pressure gas is injected into the mold through the injection nozzle to demold the mold, thereby obtaining an injection molded blank; (8) Interior decoration processing: The injection molding interface and burr position of the injection molded blank are cut and polished to obtain the interior decoration parts.

2. The injection molding production process of an automobile interior decoration part according to claim 1, characterized in that: The demoulding agent is selected from one of silicone methyl branched silicone oil, polyethylene wax, fluororesin powder and mica powder.

3. The injection molding production process of an automobile interior decoration part according to claim 1, characterized in that: The preheating temperature of the injection mold is 150-200° C., and the preheating time is 10-20 minutes.

4. The injection molding production process of an automobile interior decoration part according to claim 1, characterized in that: The injection molding raw materials are added with a heat stabilizer, a flame retardant and a modifier, and during mixing and stirring, a high-speed stirrer is used for mixing and stirring, the stirring speed is 100 r / min, the stirring time is 10-15 minutes, and the heating temperature during stirring is 100-120° C.

5. The injection molding production process of an automobile interior decoration part according to claim 1, characterized in that: The vibration machine is an ultrasonic vibration machine, and the ultrasonic vibration machine works for 3-5 seconds each time.

6. The injection molding production process of an automobile interior decoration part according to claim 1, characterized in that: After the injection molding in step (5) is completed, the mold needs to be pressure-maintained and pressure needs to be continuously applied to the inside of the mold. The applied pressure value is 50-70 kg / cm 3 , , the holding time is 40-60 minutes.

7. An injection molding production process for automotive interior decoration parts according to any one of claims 1 to 6, characterized in that: The material composition of the injection mold includes the following components in mass percentage: C: 0.30~0.40%; Si: 0.20~0.40%; Mn: 1.2~1.5%; Cr: 1.5~2.0%; Mo: 1.5~2.0%; Ni: 0.8~1.2%; V: 0.2~0.4%, and the balance is Fe.

8. The injection molding production process of an automobile interior decoration part according to claim 7, characterized in that: The Si is added in the form of ferrosilicon containing 73% Si, the Mn is added in the form of ferromanganese containing 65% Mn, the Cr is added in the form of low-carbon ferrochrome containing 57% Cr, the Mo is added in the form of molybdenum plate containing 55% Mo, the Ni is added in the form of pure nickel plate, and the V is added in the form of ferrovanadium containing 50% V.