Reinforced adhesive film and preparation method thereof

By adding reinforcement components using electrostatic flocking method on the surface of the adhesive film, the problem of uneven mixing of reinforcement components and resin matrix is ​​solved, and the film strength improvement and process simplification is achieved, which is suitable for existing production conditions and meets industrial needs.

CN119060641APending Publication Date: 2024-12-03HAIYING AEROSPACE MATERIALS RES INST (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310623892.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing film reinforcement methods, it is difficult to mix the reinforcement components with the resin matrix fully and uniformly, resulting in uneven distribution, increasing equipment input and process changes, and the reinforcement components are easily retained on the equipment, affecting production efficiency.

Method used

The reinforced film design is adopted with a thickness-direction stacked structure, and the reinforced components such as chopped fibers and carbon nanotubes are added quantitatively and uniformly to the surface of the conventional adhesive film through electrostatic flocking method to independently control the distribution of the reinforced components and the adhesive film body layer. , avoid the impact of increasing viscosity on the equipment, and achieve high-precision uniform distribution.

Benefits of technology

It realizes the uniform distribution of components on the surface of the adhesive film, improves the structural strength of the adhesive layer, simplifies the process flow, is suitable for existing production conditions, and is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060641A_ABST
    Figure CN119060641A_ABST
Patent Text Reader

Abstract

The invention discloses a reinforced adhesive film and a preparation method thereof, and relates to the technical field of composite materials, a reinforced component and an adhesive film resin system are independent in a preparation process through a laminated structure which is macroscopically presented in a thickness direction, so that the reinforced component and the adhesive film resin system are respectively controlled to realize uniform distribution, and aiming at a current goods shelf type conventional adhesive film product, the preparation method is simple and convenient. Under the condition that original conventional adhesive film production conditions are not changed, chopped fibers, carbon nanotubes, graphene and other reinforcing components are quantitatively, uniformly and quickly implanted into the surface of a conventional adhesive film through flocking operation by adopting an electrostatic flocking method after the conventional adhesive film is prepared, so that the preparation of the reinforced adhesive film is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite materials, and in particular to a reinforced adhesive film structure design and a preparation method thereof. Background Art

[0002] Adhesive film is an indispensable thin layer of resin film in the bonding of various sandwich structures and composite materials. The conventional thickness ranges from 0.1mm to 1mm. Although its high shear strength enables the bonded structure to achieve performance comparable to that of the composite material body structure, in some application environments where a larger adhesive layer thickness is formed, its performance is closer to that of the resin body, resulting in insufficient structural strength. Therefore, it is necessary to strengthen the adhesive film required for such applications and improve the body strength of the adhesive layer to ensure that the structural performance meets the design requirements.

[0003] Without significantly increasing the weight of the resin, the commonly used resin reinforcement method is to use reinforcing components such as chopped fibers, carbon nanotubes, and graphene to improve the performance of the resin matrix. The structural strength of the matrix can be significantly improved with a small weight increase (generally less than 10%). At present, the film reinforcement is usually carried out by mixing the reinforcement components in a certain ratio in the resin matrix and then preparing the film. There are three main problems: 1) The reinforcement components, whether chopped fibers, carbon nanotubes, graphene, etc., cannot be integrated with the resin matrix components. After adding, the viscosity of the resin system will be significantly increased, and it is difficult to achieve sufficient and uniform mixing, which is easy to cause uneven distribution of the reinforcement in the subsequent film, making it difficult to achieve the reinforcement effect; 2) Because the viscosity of the resin system increases after adding the reinforcement components, the resin mixing equipment and the film coating equipment need to be modified to meet the film preparation under high viscosity, which increases equipment investment and process changes, and has a great impact on the products that have been engineered; 3) After adding the reinforcement components, the reinforcement is easy to remain on the working surface of the equipment under the adhesion of the resin, and it is more difficult to clean than the resin body, which increases more preparation work when changing the preparation of different system films. Therefore, it is very necessary to develop a more universal reinforcement film structure and adopt a more process-realizable preparation method to conveniently realize the processing of traditional conventional films to obtain reinforced films. Summary of the invention

[0004] The main purpose of the present invention is to design a universal reinforced film structure, which makes the reinforcing components and the film resin system independent in the preparation process through the macroscopically presented laminated structure in the thickness direction, so as to control them separately to achieve uniform distribution. For the current conventional film products on the shelf, without changing the original conventional film production conditions, after the conventional film is prepared, the electrostatic flocking method is adopted to implant the reinforcing components such as chopped fibers, carbon nanotubes, graphene, etc. into the surface of the conventional film quantitatively, evenly and quickly through the flocking operation, thereby realizing the preparation of the reinforced film.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A reinforced adhesive film comprises an adhesive film body layer and a reinforced component layer presenting a laminated structure along the thickness direction; wherein:

[0007] The adhesive film body layer is an adhesive film made of a resin matrix through coating, and the resin matrix is ​​one of an epoxy resin system, a bismaleimide resin system, a cyanate resin system, and an unsaturated polyester resin system;

[0008] The reinforcing component layer is made of a reinforcing component selected from chopped carbon fiber, chopped aramid fiber, carbon nanotube and graphene by high-voltage electrostatic flocking method, and the reinforcing component is evenly distributed on the surface of the adhesive film body.

[0009] Furthermore, the adhesive film body layer is cured at room temperature (20-30° C.), medium temperature (60-120° C.) or high temperature (120-200° C.) after coating.

[0010] Furthermore, the adhesive film body layer is prepared by a coating method.

[0011] Furthermore, the thickness of the adhesive film body layer is 0.01-0.5 mm.

[0012] Furthermore, the film surface density in the film body layer is 10-500 g / m 2 .

[0013] Furthermore, the flocking surface density is 1%-5% of the film surface density.

[0014] Furthermore, the fiber length of the chopped carbon fiber and the chopped aramid fiber is 0.5-5 mm.

[0015] Furthermore, the carbon nanotubes and graphene are carboxylated or hydroxylated.

[0016] A method for preparing a reinforced adhesive film comprises the following steps:

[0017] 1) Selecting a film made of a resin matrix by coating, the resin matrix is ​​one of an epoxy resin system, a bismaleimide resin system, a cyanate resin system, and an unsaturated polyester resin system; the film is unrolled on a film roll, with one side facing the release paper close to the flocked negative plate, and the other side is in the flocking space;

[0018] 2) Selecting one of chopped carbon fiber, chopped aramid fiber, carbon nanotube, and graphene as a reinforcing component and placing it on the flocked positive electrode plate;

[0019] 3) The release paper enters the flocking area, and the film is flocked according to the set flocking voltage and flocking time;

[0020] 4) The flocked film is sent to the winding area and rolled up to obtain a reinforced film.

[0021] Furthermore, the flocking voltage is 10-25KV, and the flocking time is 5-30s.

[0022] Furthermore, the reinforced adhesive film protected by the release paper is obtained by rolling up, and the release paper is removed as needed during use.

[0023] Advantages of the technical solution of the present invention:

[0024] 1. The designed reinforced film with a laminated structure in the thickness direction realizes the independent distribution control of the reinforced component layer and the film body layer. Among them, the uneven distribution state of the reinforced film in the thickness direction changes with the flow of the film body when the reinforced film is used later, achieving redistribution in the thickness direction, and realizing full reinforcement of the adhesive layer between the film body layer and the reinforced component layer.

[0025] 2. The independent distribution control of the reinforcing component layer and the film body layer avoids the influence of the reinforcing component on the film preparation after increasing the viscosity of the resin system in the conventional preparation method. It has the characteristics of strong applicability. Since it has no influence on the production process of the original film, it can be applied to the shelf-type film products that have been prepared.

[0026] 3. According to the principle of electrostatic flocking, the flocking voltage and flocking time can be controlled to control the amount of reinforcing components added. In addition, since the DC high-voltage electric field used for flocking is highly uniform and easy to control, it is possible to achieve high-precision uniform distribution of reinforcing components on the flocking surface of the film. By controlling the flocking voltage and flocking time, it is possible to produce reinforced films with different reinforcing components or combinations and reinforcing component contents on one production line, and the process has strong adjustable capabilities.

[0027] 4. The DC high-voltage flocking electric field used can achieve extremely high stability, which can ensure the uniform distribution of the reinforcing components of the reinforced film on the flocking surface in continuous production, and can meet the application requirements of industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the structure of a conventional adhesive film.

[0029] Figure 2 It is a schematic diagram of the structure of a reinforced adhesive film proposed by the present invention.

[0030] Figure 3 Schematic diagram of the reinforced film prepared by the present invention.

[0031] Figure 4 These are photos of the surface structures of the enhanced adhesive film and the conventional adhesive film prepared in Example 1 of the present invention.

[0032] Figure 5 It is a performance test data chart of the reinforced adhesive film prepared in Example 1 of the present invention and the conventional adhesive film. DETAILED DESCRIPTION

[0033] In order to make the above features and advantages of the present invention more clearly understood, the following is a detailed description with reference to the accompanying drawings.

[0034] Figure 1 It is a schematic diagram of the structure of a conventional adhesive film, which is mainly composed of a conventional adhesive film made of a resin matrix coating.

[0035] Figure 2 Schematic diagram of the structure of the enhanced adhesive film proposed by the present invention, which adds a layer of reinforcing component on the basis of the conventional adhesive film. Specifically, the enhanced adhesive film comprises an adhesive film body layer and a reinforcing component layer presenting a laminated structure along the thickness direction.

[0036] The main layer of the adhesive film is a conventional adhesive film made of a resin matrix by coating and curing. The resin matrix is ​​one of epoxy resin system, bismaleimide resin system, cyanate resin system, and unsaturated polyester resin system. The curing is room temperature curing (20-30°C), medium temperature curing (60-120°C) or high temperature curing (120-200°C). The thickness of the main layer of the adhesive film is 0.01-0.5mm, and any thickness can be selected as needed. In this embodiment, the thickness is 0.1mm. The surface density of the adhesive film is 10-500g / m 2 Any surface density can be selected as needed. In this embodiment, the surface density of the film is 200 g / m 2 .

[0037] The reinforcing component layer is made of a reinforcing component selected from chopped carbon fiber, chopped aramid fiber, carbon nanotube and graphene by high-voltage electrostatic flocking method, and the reinforcing component is evenly distributed on the surface of the adhesive film body.

[0038] As a preferred embodiment, the flocking surface density is 1%-5% of the film surface density. Any ratio can be selected as needed. In this embodiment, the flocking surface density is 2% of the film surface density.

[0039] As a preferred implementation, the fiber length of the chopped carbon fiber and the chopped aramid fiber is 0.5-5 mm, and any length can be selected as needed. In this embodiment, chopped carbon fiber with a length of 3 mm is selected.

[0040] As a preferred embodiment, the carbon nanotubes and graphene can be carboxylated or hydroxylated as required.

[0041] The present invention also provides a method for preparing a reinforced adhesive film. Figure 3 As shown, the following steps are included:

[0042] 1) Selecting a film made of a resin matrix by coating, the resin matrix is ​​one of an epoxy resin system, a bismaleimide resin system, a cyanate resin system, and an unsaturated polyester resin system; the film is unrolled on a film roll, with one side facing the release paper close to the flocked negative plate, and the other side is in the flocking space;

[0043] 2) Selecting one of chopped carbon fiber, chopped aramid fiber, carbon nanotube, and graphene as a reinforcing component and placing it on the flocked positive electrode plate;

[0044] 3) The release paper enters the flocking area, and the film is flocked according to the set flocking voltage and flocking time; the flocking voltage can be selected from 10 to 25 kV, and the flocking time can be selected from 5 to 30 seconds, which needs to be determined according to actual needs.

[0045] 4) The flocked film is brought into the winding area to obtain a reinforced film protected by a release paper, and the release paper is removed as needed during use.

[0046] According to the technical solution of the present invention, three groups of embodiments are specifically implemented. The following Table 1 gives the specific parameters of the three groups of embodiments.

[0047] Table 1 Example parameters

[0048]

[0049] The surface structure morphology of the enhanced film prepared in Example 1 and the conventional film is as follows: Figure 4 As shown, (a) is a microscopic photograph of the surface structure of the reinforced film in an embodiment of the present invention, specifically a microscopic photograph of the surface structure of the reinforced film treated with 1% carbon nanotube flocking reinforcement; (b) is a microscopic photograph of the surface structure of a conventional film.

[0050] The performance test data of the enhanced film prepared in Example 1 and the conventional film are as follows: Figure 5 As shown, (a) is a comparison of the structural bearing capacity of the adhesive film reinforced with 1% carbon nanotube content and the unreinforced adhesive film, indicating that the lateral pressure bearing load of the reinforced adhesive film honeycomb sandwich structure is significantly improved; (b) is a comparison of the structural strength of the adhesive film reinforced with different contents of carbon nanotube fiber flocking, indicating that the reinforced adhesive films with different contents have significantly improved the lateral pressure performance of the honeycomb sandwich structure compared with the unreinforced adhesive film.

[0051] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Appropriate modifications or equivalent substitutions of the technical solutions of the present invention made by ordinary technicians in the field should all be included in the protection scope of the present invention. The protection scope of the present invention shall be based on what is defined in the claims.

Claims

1. A reinforced film, characterized in that: It includes a film body layer and a reinforcement component layer showing a laminated structure along the thickness direction; wherein, The adhesive film body layer is an adhesive film made of a resin matrix through coating, and the resin matrix is ​​one of an epoxy resin system, a bismaleimide resin system, a cyanate resin system, and an unsaturated polyester resin system; The reinforcing component layer is made of a reinforcing component selected from chopped carbon fiber, chopped aramid fiber, carbon nanotube and graphene by high-voltage electrostatic flocking method, and the reinforcing component is evenly distributed on the surface of the adhesive film body.

2. The reinforced adhesive film according to claim 1, characterized in that: The main layer of the adhesive film is cured at room temperature, medium temperature or high temperature after coating.

3. The reinforced adhesive film according to claim 1, characterized in that: The main layer of the adhesive film is prepared by a coating method.

4. The reinforced adhesive film according to claim 1, characterized in that: The thickness of the main layer of the adhesive film is 0.01-0.5 mm.

5. The reinforced adhesive film according to claim 1, characterized in that: The film surface density in the film body layer is 10-500g / m 2 .

6. The reinforced adhesive film according to claim 5, characterized in that: The flocking surface density is 1%-5% of the film surface density.

7. The reinforced adhesive film according to claim 1, characterized in that: The fiber length of the chopped carbon fiber and the chopped aramid fiber is 0.5-5 mm.

8. The reinforced adhesive film according to claim 1, characterized in that: The carbon nanotubes and graphene are carboxylated or hydroxylated.

9. A method for preparing the enhanced adhesive film according to any one of claims 1 to 8, characterized in that: The following steps are involved: 1) Selecting a film made of a resin matrix by coating, the resin matrix is ​​one of an epoxy resin system, a bismaleimide resin system, a cyanate resin system, and an unsaturated polyester resin system; the film is unrolled on a film roll, with one side facing the release paper close to the flocked negative plate, and the other side is in the flocking space; 2) Selecting one of chopped carbon fiber, chopped aramid fiber, carbon nanotube, and graphene as a reinforcing component and placing it on the flocked positive electrode plate; 3) The release paper enters the flocking area, and the film is flocked according to the set flocking voltage of 10-25KV and flocking time of 5-30s; 4) The flocked film is sent to the winding area and rolled up to obtain a reinforced film.