Ultra-wide-temperature stable sodium bismuth titanate-based dielectric ceramic material and preparation method thereof

By introducing Ca(Fe0.5Ta0.5)O3 into the sodium bismuth titanate matrix, adjusting the dielectric anomaly peak, expanding the temperature and stability interval of dielectric ceramic materials, solving the decline in the performance of existing barium titanate-based materials at high temperatures Problem, ultra-wide temperature stability with high dielectric constant and low dielectric loss is achieved.

CN119069259AActive Publication Date: 2024-12-03CENT SOUTH UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411172266.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing barium titanate-based dielectric ceramic capacitors show problems such as decreased capacity, increased loss, reduced temperature stability and voltage resistance in high-temperature environments, and it is difficult to meet the needs of extreme environments of high and low temperatures.

Method used

By using the doping/solid solution modification method, the relative content and size of polar nano micro-domain are changed by introducing Ca(Fe0.5Ta0.5)O3 into the matrix of bismuth sodium titanate (Bi0.5Na0.5TiO3) to change the relative content and size of polar nano micro-domain to adjust the The dielectric anomaly peak extends the dielectric stability range below -100℃ and above 400℃, forming ultra-wide temperature stable ceramic materials with high dielectric constant and low dielectric loss.

Benefits of technology

It achieves excellent dielectric properties with a dielectric constant change rate of less than 15% and a dielectric loss of less than 0.02 in the temperature range of -150~450℃, which significantly expands the temperature stability range of dielectric ceramic materials and is suitable for extreme environments of high and low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069259A_ABST
    Figure CN119069259A_ABST
Patent Text Reader

Abstract

The invention discloses an ultra-wide-temperature stable sodium bismuth titanate-based dielectric ceramic material and a preparation method thereof, the chemical formula of the ultra-wide-temperature stable sodium bismuth titanate-based dielectric ceramic material is (1-x) (0.94 Bi0. 5Na0. 5TiO3-0.06 BaTiO3)-xCa (Fe0. 5Ta0. 5) O3, and x ranges from 0.18 to 0.22. The invention also discloses a preparation method of the ultra-wide-temperature stable sodium bismuth titanate-based dielectric ceramic material. The sodium bismuth titanate-based dielectric ceramic material is prepared by a traditional solid phase method, and has excellent dielectric properties and temperature stability: the room temperature dielectric constant at 1kHz is 670, the dielectric loss is as low as 0.0037, the change rate of the dielectric constant in the temperature range of-150 to 450 DEG C is less than 15%, and the dielectric loss in the temperature range of-110 to 300 DEG C is less than 0.02. The ultra-wide-temperature stable sodium bismuth titanate-based dielectric ceramic material provided by the invention is suitable for being used in ceramic dielectric capacitors in high and low temperature extreme environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lead-free dielectric ceramics, and in particular relates to an ultra-wide temperature stable sodium bismuth titanate-based dielectric ceramic material and a preparation method thereof. Background Art

[0002] Dielectric ceramic capacitors are widely used in automotive electronics, consumer electronics, aerospace, weapons and equipment due to their high capacitance, compact size, and good frequency, temperature and withstand voltage characteristics. In some scenarios, dielectric ceramic capacitors will face extreme working conditions such as high temperature, severe cold, high pressure, and high impact, which puts extremely high demands on the high and low temperature stability of the dielectric properties of key dielectric ceramic materials. For example, related electronic devices in aircraft and automobile engine monitoring systems may need to withstand high temperatures of 300 to 600°C. At present, commercial high-capacity dielectric ceramic capacitors mainly use barium titanate as raw material, and the operating temperature range of the prepared devices is limited to -55 to 200°C. Due to the low Curie temperature of barium titanate (~120°C), the upper limit of the operating temperature is difficult to break. Once the temperature exceeds 200°C, the capacity of the capacitor decreases, the loss increases, and the temperature stability, withstand voltage characteristics and reliability are significantly reduced. Therefore, it is urgent to develop new dielectric ceramic materials with a wider operating temperature range to meet more extreme high and low temperature working environments.

[0003] Sodium bismuth titanate (Bi 0.5 Na 0.5 TiO3 (BNT) is a type of relaxor ferroelectric with a perovskite structure. There are two unique dielectric anomaly peaks in its dielectric temperature spectrum, namely, T s (~200℃, dielectric constant ~1500) hump and T m The maximum dielectric constant peak at (~320℃, dielectric constant ~3000) is conducive to achieving wide temperature stabilization of the dielectric constant. The dielectric anomaly of BNT originates from the thermal evolution of the trigonal R3c and tetragonal P4bm polar nano-microdomains with similar free energy in the material on a local scale. If doping / solid solution modification is used, the relative content, size or polarization ability of the polar nano-microdomains can be changed to increase the T s By moving the dielectric to below room temperature and suppressing the dielectric anomaly peak, it is expected that the T s -T m A flat and wide dielectric temperature curve is obtained in the temperature range. However, due to the T s It is too high to 200℃, and it is difficult to extend the low temperature section of the metastable range to below -100℃ in BNT-based ceramics. On the other hand, the T m ~320℃, so it is also very challenging to extend the high temperature end of the metastable range to above 400℃. Summary of the invention

[0004] In view of the shortcomings of the prior art, the first object of the present invention is to provide a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability having a high dielectric constant and low dielectric loss, and at the same time, the dielectric properties have very excellent temperature stability. The sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability provided by the present invention is suitable for use in ceramic dielectric capacitors under high and low temperature extreme environments.

[0005] The second object of the present invention is to provide a method for preparing the above-mentioned ultra-wide temperature stable sodium bismuth titanate-based dielectric ceramic material. The present invention adopts a traditional solid phase method, and the preparation process is simple and controllable.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention discloses a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability. The sodium bismuth titanate-based dielectric ceramic material has a chemical formula of (1-x)(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-xCa(Fe 0.5 Ta 0.5 )O3, wherein x is 0.18-0.22, preferably 0.20.

[0008] The sodium bismuth titanate-based dielectric ceramic material provided by the present invention, 0.94Bi 0.5 Na 0.5 There are two dielectric anomaly peaks in the TiO3-0.06BaTiO3 matrix, namely T s The hump at s ~100℃) and T m The maximum dielectric constant peak (T m ~260℃). Doped with Ca(Fe 0.5 Ta 0.5 )O3, Ca 2+ ions enter the A site of the perovskite structure and interact with the Bi 3+ 、Na + and Ba 2+ Ion coexistence; Fe 3+ and Ta 5+ The ions enter the B site of the perovskite structure and interact with the Ti 4+ Ion coexistence: Whether at the A or B position, the coexistence of cations with different valence states and ionic radii leads to a significant enhancement of the random field in the material, the destruction of the long-range ferroelectric ordered structure, the appearance of a nanodomain structure, and the decrease in the size of the polar region and the decrease in the degree of coupling, which significantly enhances the dielectric relaxation of the ceramic, which is reflected in the broadening and depression of the dielectric peak in the dielectric temperature spectrum. When x is 0.18-0.22, T s has dropped to about -150℃, T mIt is difficult to identify, forming a flat and low dielectric constant platform, extending the low-temperature end and high-temperature end of the metastable range to below -100°C and above 400°C, respectively.

[0009] The sodium bismuth titanate-based dielectric ceramic material provided by the invention has a high dielectric constant of 670 and a low dielectric loss of 0.0037 at room temperature, and a dielectric constant change rate of less than 15% within a temperature range of -150 to 450° C., and a dielectric loss of less than 0.02 within a temperature range of -110 to 300° C.

[0010] The sodium bismuth titanate-based dielectric ceramic material provided by the present invention, Ca(Fe 0.5 Ta 0.5 The solid solubility of )O3 has an important influence on the room temperature dielectric constant, dielectric constant and temperature stability of the sodium bismuth titanate-based dielectric ceramic material. When the solid solubility is controlled to be 18-22 mol%, it can unexpectedly show excellent performance. The study found that below the lower limit, the room temperature dielectric constant and dielectric loss are high, and the temperature stability of the dielectric performance is poor; and when the solid solubility is too high, it will lead to the appearance of impurity phases in the ceramic.

[0011] Preferably, the tetragonal P4bm phase, the orthorhombic Pnma phase and the trigonal R3c phase coexist in the sodium bismuth titanate-based dielectric ceramic material;

[0012] The grains of the sodium bismuth titanate-based dielectric ceramic material contain a blocky nanodomain structure;

[0013] The grain size of the sodium bismuth titanate-based dielectric ceramic material is 1.79-2.37 μm.

[0014] The sodium bismuth titanate-based dielectric ceramic material provided by the present invention, Ca(Fe 0.5 Ta 0.5 )O3 doped with 0.94Bi 0.5 Na 0.5 After the TiO3-0.06BaTiO3 matrix is ​​doped, the random field in the ceramic is significantly enhanced due to the diversity of ion valence and ion radius, destroying the long-range ferroelectric ordered structure and forming a nanodomain structure. 0.5 Na 0.5 There is a tetragonal P4bm phase (accounting for about 97.7wt%, a 0 a 0 c + type oxygen octahedron tilted) and trigonal R3c phase (about 2.3wt%, a - a - a - type oxygen octahedron tilted), while Ca(Fe 0.5 Ta 0.5The incorporation of )O3 significantly decreased the perovskite structural tolerance factor from 0.984 (x = 0) to 0.962 (x = 0.20), inducing a 0 a 0 c + The inclined tetragonal P4bm oxygen octahedron faces a - a - c + The orthorhombic Pnma phase of the tilted oxygen octahedron transforms and finally obtains a three-phase coexistence structure. In the x=0.20 ceramic, the content of the tetragonal P4bm phase is 58.8wt%, the content of the orthorhombic Pnma phase is 33.3wt%, and the content of the trigonal R3c phase is 7.9wt%. The multi-phase coexistence and nano-domain structure promote the ceramic to show the characteristics of diffuse phase transition with temperature, making its dielectric properties have excellent temperature stability.

[0015] The present invention also provides a method for preparing an ultra-wide temperature stable sodium bismuth titanate-based dielectric ceramic material, according to (1-x)(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-xCa(Fe 0.5 Ta 0.5 )O3 is prepared by mixing raw material powders in a stoichiometric ratio of the elements, and the mixed material A is obtained by the first ball milling. The mixed material A is pre-fired to obtain pre-fired powder. The pre-fired powder is ball milled for a second time to obtain a mixed material B. The mixed material B is granulated to obtain granulated powder. The granulated powder is pressed into a green body, and the green body is debinded and sintered to obtain a sodium bismuth titanate-based dielectric ceramic material.

[0016] The technical solution of the present invention is simple and controllable, with low cost. The traditional solid phase method is adopted, and after one pre-firing, an ultra-wide temperature stable sodium bismuth titanate-based dielectric ceramic material can be obtained. The method of the present invention can prepare a large amount of ceramic powder at one time, with a large output, and the prepared ceramic powder has no agglomeration and good filling property.

[0017] The preferred solution is based on (1-x)(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-xCa(Fe 0.5 Ta 0.5 )O3 is made of Bi2O3, Na2CO3, BaCO3, CaCO3, TiO2, Fe2O3 and Ta2O5 in a stoichiometric ratio of elements.

[0018] In the actual operation process, in order to ensure the accuracy of the experiment, some raw materials that are easy to absorb moisture must be dried before weighing. For example, before weighing, take an appropriate amount of Na2CO3 powder and dry it at 200℃ on a temperature-controlled magnetic stirrer for 3 hours. And weigh it quickly at the end to reduce the absorption of moisture in the air.

[0019] In addition, the raw materials are calculated according to the chemical formula, and the required drug mass is weighed with an electronic balance and placed in a ball mill. The amount of the substance has a great influence on the performance of the ceramic, so the weighing should be accurate to three decimal places.

[0020] In a preferred embodiment, the rotation speed of the first ball milling is 200 to 300 rpm, and the time of the first ball milling is 12 to 24 hours.

[0021] In a preferred embodiment, the first ball milling is wet ball milling, and the ball milling medium is anhydrous ethanol, wherein the mass ratio of the raw material powder, anhydrous ethanol, and ball milling balls is 1:1:3-5.

[0022] During the first ball milling, the mass ratio of the raw material powder, anhydrous ethanol and ball milling balls is controlled within the range of the present invention, and the raw material powder can be fully mixed and refined by controlling the ball milling speed and time, thereby promoting a more complete subsequent reaction.

[0023] In the actual operation process, the raw materials, anhydrous ethanol and zirconium balls are poured into the ball mill in proportion, and no impurities are introduced into the ball mill. A planetary ball mill is used, and the ball mill is sealed and fixed in the ball mill. After ball milling, the ball mill is taken out and dried in a drying oven at 70°C for 24 to 36 hours until the powder is completely dry and then passed through a 150-mesh sieve to completely separate the powder and the zirconium balls to obtain a mixed material A.

[0024] In a preferred embodiment, after the first ball milling is completed, the obtained ball milled powder is dried and then sieved through a 150-mesh sieve to obtain a mixed material A.

[0025] In a preferred embodiment, the pre-sintering process is as follows: the mixed material A is heated to 850-950°C at a heating rate of 3-8°C / min in an air atmosphere, kept at this temperature for 2-5 hours, and then cooled in the furnace. In order to allow the powder materials to react fully, pre-sintering is first performed to initially obtain pre-sintered powder.

[0026] In a preferred embodiment, the rotation speed of the second ball milling is 400-600 rpm, and the time of the second ball milling is 8-12 hours.

[0027] In a preferred embodiment, the second ball milling is wet ball milling, and the ball milling medium is anhydrous ethanol, wherein the mass ratio of the calcined powder, anhydrous ethanol, and ball milling balls is 15:20:45-60.

[0028] In the present invention, due to the complex composition of the ceramic system, the present invention adopts a higher ball milling speed on the one hand, and on the other hand, controls the mass ratio of pre-fired powder, anhydrous ethanol, and ball milling balls to obtain fine powder with a particle size distribution of 300 to 500 nm, and further makes the composition of the pre-fired powder uniform, which is ultimately beneficial to the subsequent sintering densification. Therefore, it is necessary to control the ball milling speed, etc. If the ball milling speed is too slow, it will lead to lower sintering activity, and may also cause component segregation in the fired ceramic, thereby deteriorating the ceramic performance.

[0029] In the actual operation process, the pre-burned powder, anhydrous ethanol and zirconium balls are poured into the ball mill in proportion, and no impurities are introduced into the ball mill. A planetary ball mill is used, and the ball mill is sealed and fixed in the ball mill. After ball milling, the ball mill is taken out and dried in a drying oven at 70°C for 24 to 36 hours until the powder is completely dry and then passed through a 200-mesh sieve to completely separate the powder and the zirconium balls to obtain a mixed material B.

[0030] In a preferred embodiment, after the second ball milling is completed, the obtained ball milled powder is dried and then sieved through a 200-mesh sieve to obtain a mixed material B.

[0031] In a preferred embodiment, the process of granulating the mixed material B is as follows: a binder is added to the mixed material B and then the mixed material B is ground into granules, wherein the amount of the binder added is 3-5% of the mass of the mixture.

[0032] The binder can be a substance with adhesive properties well known in the granulation industry; preferably, polyvinyl butyral.

[0033] In a preferred embodiment, the pressing pressure is 20-30 MPa, and the holding time is 3-8 min.

[0034] In the actual operation process, 0.3-0.5 g of granulated powder is poured into a mold with a diameter of 10 mm for pressing and then the pressed green body is subjected to debinding and sintering treatments in an air atmosphere.

[0035] Preferably, the debinding sintering process is: firstly heat up to the debinding temperature of 550-650°C at a heating rate of 0.5-2°C / min and keep warm for 2-4h, then heat up to the sintering temperature of 1160-1200°C at a rate of 3-8°C / min and keep warm for 2-4h.

[0036] Beneficial effects of the present invention:

[0037] (1) The present invention provides a sodium bismuth titanate-based dielectric ceramic material having excellent dielectric properties and temperature stability, wherein the second component Ca(Fe 0.5 Ta 0.5 )O3,0.94Bi 0.5 Na 0.5The room-temperature dielectric loss of the TiO3-0.06BaTiO3 ceramic system has been greatly suppressed, and a relatively high room-temperature dielectric constant has been maintained; more importantly, the temperature-stable range of dielectric properties has been greatly widened, and the relatively high dielectric constant and extremely low dielectric loss remain stable over an ultra-wide temperature range.

[0038] (2) The 0.80 (0.94 Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 )O3 ceramics, the dielectric constant is 670 at room temperature 25℃, the dielectric loss is as low as 0.0037, the change rate of the dielectric constant in the temperature range of -150~450℃ is less than 15%, and the dielectric loss in the temperature range of -110~300℃ is less than 0.02.

[0039] (3) The raw materials used in the present invention do not contain rare earth elements and precious metal elements, so the cost is low; and the raw materials do not contain lead, so they are harmless to the environment.

[0040] (4) The present invention extends the low temperature end of the dielectric ceramic temperature stability range to -150°C and the high temperature end to 450°C, which is significantly better than commercial barium titanate-based dielectric ceramic materials and the currently reported sodium bismuth titanate-based dielectric ceramic materials, and has great application prospects in high and low temperature dielectric ceramic capacitors. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 , in Example 1, 0.80 (0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 )X-ray diffraction patterns and phase structure refinement results of O3 ceramics.

[0042] Figure 2 , in Example 1, 0.80 (0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 )Scanning electron microscope image and particle size distribution of O3 ceramics.

[0043] Figure 3 , in Example 1, 0.80 (0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5) Low-magnification transmission electron micrograph of O3 ceramics.

[0044] Figure 4 , in Example 1, 0.80 (0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 ) Dielectric properties test diagram of O3 ceramics, where Figure 4 (a) is the dielectric temperature spectrum, Figure 4 (b) Δε obtained using dielectric temperature spectrum r / ε r25 ℃ vs. T spectrum. DETAILED DESCRIPTION

[0045] Example 1

[0046] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.

[0047] Embodiment 1 of the present invention provides an ultra-wide temperature stable sodium bismuth titanate-based dielectric ceramic material and a preparation method thereof, wherein the chemical formula is 0.80 (0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 )O3.

[0048] 0.80(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 ) Preparation of O3 ceramic materials

[0049] Bi2O3, Na2CO3, BaCO3, CaCO3, TiO2, Fe2O3 and Ta2O5 raw materials were weighed respectively according to the molar ratio of 0.188:0.188:0.048:0.2:0.8:0.05:0.05. Before weighing, the Na2CO3 powder was dried at 200°C for 3 h on a temperature-controlled magnetic stirrer. The raw materials were placed in a ball mill with zirconium oxide balls and anhydrous ethanol as the medium. The mass ratio of the raw materials, anhydrous ethanol and zirconium balls was 1:1:3. The raw materials were placed in a planetary ball mill and ball-milled at 250 rpm for 18 h. The ball mill was taken out, dried at 70°C for 24 h, and passed through a 150-mesh sieve to obtain a mixed material A. The mixed material A was heated to 900°C at a heating rate of 5°C / min in an air atmosphere. After being kept warm for 3 h, it was cooled in the furnace to obtain a pre-sintered powder. The pre-burned powder, anhydrous ethanol and zirconium balls were poured into a ball mill at a ratio of 15:20:45, placed in a planetary ball mill, ball-milled at 400 rpm for 12 hours, and then dried at 70°C for 24 hours, and passed through a 200-mesh sieve to obtain a mixed material B. Add 3% polyvinyl butyral by mass to the mixed material B, grind it thoroughly until the powder is granular, and obtain granulated powder with uniform particles. Take 0.3g of granulated powder and press it into a cylindrical green body with a diameter of about 10mm at a pressure of 20Mpa for 5 minutes. The green body was placed in an alumina crucible and buried with pre-burned powder of the same composition. First, the temperature was increased to 600°C at a rate of 1°C / min and kept for 2 hours to remove the binder, and then the temperature was increased to 1180°C at a rate of 5°C / min and kept for 3 hours to sinter, and naturally cooled with the furnace to obtain 0.80 (0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 )O3 ceramic material.

[0050] 0.80(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.20Ca(Fe 0.5 Ta 0.5 ) Characterization of O3 Ceramic Materials

[0051] Structural characterization: First, the crystal phase is detected by X-ray diffraction analysis (XRD). Figure 1 As shown, it can be seen that the prepared ceramic material is a pure perovskite structure without impurity phases. After phase structure refinement, it was found that tetragonal P4bm phase, orthorhombic Pnma phase and trigonal R3c phase coexist in the ceramic, and the content of each phase is 58.8wt%, 33.3wt% and 7.9wt% respectively.

[0052] The obtained ceramic material was subjected to scanning electron microscopy (SEM) testing. Before testing, the ceramic was polished and thermally etched. Figure 2It can be seen that the prepared ceramics have no obvious defects, good crystallinity, uniform grain size and an average grain size of about 2.08 μm.

[0053] The obtained ceramic material was examined by transmission electron microscopy (TEM). Figure 3 It can be seen that there are bulk nanodomain structures in the ceramic grains.

[0054] Dielectric property characterization: The sintered ceramic was polished to a thickness of 0.5 mm, medium-temperature silver paste was coated on both sides, and the silver electrode was fired at 550°C for 30 minutes. The dielectric temperature spectrum test uses a high-temperature impedance analyzer to test the dielectric constant ε of the ceramic. r The dielectric loss tanδ and the change curves with temperature T and frequency f. In this test, the test temperature range is -160~450℃, and the test frequencies include 1kHz, 10kHz, 100kHz and 1MHz. Then, the measured dielectric temperature spectrum is used to calculate Δε at 1kHz. r / ε r25 The temperature stability of the dielectric constant of ceramics is evaluated by measuring the change of (dielectric constant at a certain temperature point - dielectric constant at 25°C) / dielectric constant at 25°C) with temperature.

[0055] Figure 4 (a) is the dielectric temperature spectrum of the ceramic, showing obvious dielectric peak broadening and frequency dispersion, proving the existence of temperature-dependent diffuse phase transition in the ceramic. The room temperature dielectric constant is 670 at 1 kHz, the dielectric loss is as low as 0.0037, and the dielectric loss is less than 0.02 in the temperature range of -110 to 300 °C; (b) is the Δε at 1 kHz obtained using the dielectric temperature spectrum. r / ε r25 From the ℃ vs. T graph, we can see that the temperature stability of the ceramic dielectric constant is very good, and the change rate of the dielectric constant in the temperature range of -150 to 450℃ is less than 15%.

[0056] Example 2

[0057] Compared with Example 1, the only difference is that Ca(Fe 0.5 Ta 0.5 )O3 solid solution is 22 mol%, that is, the chemical formula is 0.78 (0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.22Ca(Fe 0.5 Ta 0.5)O3, the prepared ceramic is still a pure perovskite structure, without impurity phase, the ceramic crystal phase composition is 49.9wt% P4bm phase, 41.5wt% Pnma phase and 8.6wt% R3c phase, the average grain size is 2.37μm. The room temperature dielectric constant is 635 at 1kHz, the dielectric loss is as low as 0.0035, the temperature range of dielectric loss less than 0.02 is -115~300℃, and the temperature range of dielectric constant change rate less than 15% is -158~450℃.

[0058] Comparative Example 1:

[0059] Compared with Example 1, the only difference is that no solid solution of Ca(Fe 0.5 Ta 0.5 )O3, the chemical formula is 0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3, the prepared ceramic is still a pure perovskite structure, without impurity phase, the ceramic crystal phase composition is 97.7wt% P4bm phase and 2.3wt% R3c phase, the average grain size is 1.26μm. The room temperature dielectric constant is 2040 at 1kHz, the dielectric loss is as high as 0.065, the temperature range of dielectric loss less than 0.02 is 128~400℃, and the temperature range of dielectric constant change rate less than 15% is only 105~185℃.

[0060] Comparative Example 2:

[0061] Compared with Example 1, the only difference is that Ca(Fe 0.5 Ta 0.5 )O3 solid solution is 10 mol%, that is, the chemical formula is 0.90(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-0.10Ca(Fe 0.5 Ta 0.5 )O3, the prepared ceramic is still a pure perovskite structure, without impurity phase, the ceramic crystal phase composition is 86.8wt% P4bm phase, 12.8wt% Pnma phase and 0.4wt% R3c phase, the average grain size is 1.64μm. The room temperature dielectric constant is 1082 at 1kHz, the dielectric loss is as high as 0.030, the temperature range of dielectric loss less than 0.02 is 140-335℃, and the temperature range of dielectric constant change rate less than 15% is 85-375℃.

[0062] Comparative Example 3:

[0063] Compared with Example 1, the only difference is that Ca(Fe 0.5 Ta 0.5 )O3 solid solution is 25 mol%, that is, the chemical formula is 0.75(0.94Bi0.5 Na 0.5 TiO3-0.06BaTiO3)-0.25Ca(Fe 0.5 Ta 0.5 )O3, obvious impurity phase appears in the prepared ceramics.

Claims

1. An ultra-wide temperature stable sodium bismuth titanate-based dielectric ceramic material, characterized in that: The sodium bismuth titanate-based dielectric ceramic material, Its chemical formula is (1-x)(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-xCa(Fe 0.5 Ta 0.5 )O3, where x is 0.18-0.

22.

2. The sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 1, characterized in that: The tetragonal P4bm phase, the orthorhombic Pnma phase and the trigonal R3c phase coexist in the sodium bismuth titanate-based dielectric ceramic material; The grains of the sodium bismuth titanate-based dielectric ceramic material contain a blocky nanodomain structure; The grain size of the sodium bismuth titanate-based dielectric ceramic material is 1.79-2.37 μm.

3. The method for preparing a sodium bismuth titanate-based dielectric ceramic material having an ultra-wide temperature stability according to claim 1 or 2, characterized in that: According to (1-x)(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-xCa(Fe 0.5 Ta 0.5 )O3 is prepared by mixing raw material powders in a stoichiometric ratio of the elements, and the mixed material A is obtained by the first ball milling. The mixed material A is pre-fired to obtain pre-fired powder. The pre-fired powder is ball milled for a second time to obtain a mixed material B. The mixed material B is granulated to obtain granulated powder. The granulated powder is pressed into a green body, and the green body is debinded and sintered to obtain a sodium bismuth titanate-based dielectric ceramic material.

4. The method for preparing a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 3, characterized in that: According to (1-x)(0.94Bi 0.5 Na 0.5 TiO3-0.06BaTiO3)-xCa(Fe 0.5 Ta 0.5 )O3 is made of Bi2O3, Na2CO3, BaCO3, CaCO3, TiO2, Fe2O3 and Ta2O5 in a stoichiometric ratio of elements.

5. The method for preparing a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 3, characterized in that: The rotation speed of the first ball milling is 200-300 rpm, and the time of the first ball milling is 12-24 hours; The first ball milling is wet ball milling, and the ball milling medium is anhydrous ethanol, wherein the mass ratio of raw material powder, anhydrous ethanol, and ball milling balls is 1:1:3-5; After the first ball milling is completed, the ball milled powder is dried and then sieved through a 150-mesh sieve to obtain a mixed material A.

6. The method for preparing a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 3, characterized in that: The pre-sintering process is as follows: heating the mixed material A to 850-950° C. at a heating rate of 3-8° C. / min in an air atmosphere, keeping the temperature for 2-5 hours, and then cooling the mixed material in the furnace.

7. The method for preparing a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 3, characterized in that: The second ball milling has a rotation speed of 400 to 600 rpm and a time of 8 to 12 hours; The second ball milling is wet ball milling, and the ball milling medium is anhydrous ethanol, wherein the mass ratio of the calcined powder, anhydrous ethanol, and ball milling balls is 15:20:45-60; After the second ball milling is completed, the obtained ball milled powder is dried and then sieved through a 200-mesh sieve to obtain a mixed material B.

8. The method for preparing a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 3, characterized in that: The process of granulating the mixed material B is as follows: after adding a binder to the mixed material B, the mixed material B is ground into granules, and the amount of the binder added is 3-5% of the mass of the mixed material B.

9. The method for preparing a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 3, characterized in that: The pressure of the pressing molding is 20-30 MPa, and the holding time is 3-8 minutes.

10. The method for preparing a sodium bismuth titanate-based dielectric ceramic material with ultra-wide temperature stability according to claim 3, characterized in that: The debinding sintering process is: firstly heating up to a debinding temperature of 550-650°C at a heating rate of 0.5-2°C / min and keeping the temperature for 2-4h, then heating up to a sintering temperature of 1160-1200°C at a rate of 3-8°C / min and keeping the temperature for 2-4h.

Citation Information

Patent Citations

  • Ternary system sodium-bismuth titanate lead-free piezoelectric ceramics

    CN101200370A

  • Piezoelectric ceramic composition

    CN101274850A

  • Sodium bismuth titanate-sodium tantanate solid solution ceramic material and preparation method and application thereof

    CN110436920A

  • Sodium bismuth titanate-based ceramic material with high energy storage density under low electric field and preparation method of sodium bismuth titanate-based ceramic material

    CN117285347A

  • Low temperature sintering multielement multiphase complex microwave medium ceramic and its preparation method

    CN1513808A