Negative electrode for all-solid-state battery including metal
By forming a metal nanowire entangled pore coating on the negative electrode current collector of the all-solid state battery and filling the negative electrode material, the problem of disengagement caused by volume changes in the silicon-based negative electrode active material during charging and discharging is solved, and the conductivity of the negative electrode is improved and Adhesion strength improves the charging and discharging efficiency of the battery.
Patent Information
- Application Number
- CN202311189490.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2023-09-15
- Publication Date
- 2024-12-03
AI Technical Summary
The volume change of silicon-based negative electrode active substance during charging and discharging leads to disengagement from the negative electrode current collector, and has a low conductivity, limiting the charging and discharging efficiency, and increasing the content of adhesive or conductive material will reduce battery capacity and lithium ion conductivity.
A pore coating formed by entanglement of metal nanowires is formed on the negative electrode current collector, and the coating is filled with negative electrode material to improve the adhesive strength and electrical conductivity of the negative electrode layer and the current collector.
The bonding strength between the negative electrode layer and the current collector is enhanced, the resistance is reduced, the conductivity and charging and discharging efficiency of the negative electrode are improved, the amount of conductive material is reduced, and the separation of the silicon-based negative electrode active material is prevented.
Smart Images

Figure CN119069713A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an anode for an all-solid-state battery and a method for manufacturing the same, the anode having a coating layer on an anode current collector and including pores formed by entanglement of metal nanowires. Background Art
[0002] All-solid-state batteries have attracted great attention due to their excellent stability and high energy density. The electrodes of all-solid-state batteries have a form including active materials, solid electrolytes, conductive materials, binders, etc.
[0003] Research on the application of silicon-based positive active materials to increase the capacity of all-solid-state batteries is actively underway. However, during the charging and discharging process, the volume of the silicon-based negative active material changes greatly, so detachment may occur between the negative active material and the negative current collector. In addition, compared with carbon-based negative active materials and metal-based negative active materials, silicon-based negative active materials have low electrical conductivity, which limits the migration of electrons during charging and discharging, so they have poor charging and discharging efficiency.
[0004] In order to prevent the silicon-based negative electrode active material from being separated due to such a change in the volume of the silicon-based negative electrode active material, it is possible to consider increasing the content of the binder. However, when the content of the binder increases, the resistance of the negative electrode increases, the content of the negative electrode active material and the solid electrolyte is relatively reduced, and therefore, the capacity of the negative electrode is reduced and the lithium ion conductivity of the negative electrode is reduced.
[0005] In order to compensate for the low conductivity of the silicon-based negative electrode active material, it is possible to consider increasing the content of the conductive material. However, when the content of the conductive material increases, the conductive material particles may aggregate, and thus the dispersibility of the components in the negative electrode may decrease.
[0006] The above information disclosed in this background section of the present invention is only for increasing understanding of the background of the present invention and therefore it may contain information that does not constitute the prior art that is known to ordinary technicians in this field. Summary of the invention
[0007] In a preferred aspect, the present invention provides an anode for an all-solid-state battery having excellent bonding strength between an anode layer and an anode current collector, and a method for manufacturing the same.
[0008] The term "all-solid-state battery" as used herein refers to a rechargeable secondary battery that includes an electrolyte in a solid state for transferring ions between electrodes of the battery.
[0009] In a preferred aspect, a negative electrode for an all-solid-state battery having excellent conductivity and a method for manufacturing the same are provided.
[0010] In one aspect, the present invention provides a negative electrode suitable for an all-solid-state battery, wherein the negative electrode comprises a negative electrode current collector, a coating layer disposed on the negative electrode current collector and comprising pores formed by metal nanowires, and a negative electrode layer disposed on the coating layer and comprising a negative electrode material.
[0011] In one aspect, pores are formed by entangling metal nanowires.
[0012] The coating may include a first layer configured to contact the negative electrode current collector, and a second layer disposed on the first layer and configured so that the pores are filled with a portion of the negative electrode material of the negative electrode layer. For example, about 1 wt %, about 5 wt %, about 10 wt %, about 20 wt %, about 30 wt %, about 40 wt %, about 50 wt %, about 60 wt %, about 70 wt %, about 80 wt %, about 90 wt % or about 95 wt % of the negative electrode material of the negative electrode layer may fill the pores of the coating.
[0013] The metal nanowires may suitably include nickel (Ni), copper (Cu), or a combination thereof.
[0014] The metal nanowires may suitably have a length of about 5 μm to 25 μm and a diameter of about 10 nm to 50 nm.
[0015] The thickness of the negative electrode layer may be greater than the thickness of the second layer.
[0016] The thickness of the negative electrode layer may suitably be about 25 μm to 30 μm.
[0017] The thickness of the first layer may suitably be about 6 μm to 10 μm.
[0018] The thickness of the second layer may suitably be about 5 μm to 10 μm.
[0019] The negative electrode material may include a silicon-based negative electrode active material and a solid electrolyte.
[0020] In one aspect, the present invention provides a method for manufacturing a negative electrode for an all-solid-state battery. The method comprises the following steps: preparing a solution including a precursor of metal nanowires; obtaining an intermediate by applying the solution on a negative electrode current collector; obtaining a coating layer including pores formed by forming metal nanowires on the negative electrode current collector by heat treating the intermediate; and forming a negative electrode layer by applying a slurry including a negative electrode material onto the coating layer.
[0021] The metal nanowires on the negative electrode current collector can be entangled by heat treatment.
[0022] The solution may preferably be alkaline.
[0023] The solution may also include a reducing agent.
[0024] In the process of obtaining the coating, the intermediate body may be heat treated at a temperature equal to or greater than about 120°C but less than about 140°C.
[0025] The intermediate may be heat treated for a period of time longer than about 10 hours but equal to or less than about 12 hours.
[0026] In addition, in one aspect, an all-solid-state battery comprising the negative electrode as described herein is provided.
[0027] There is also provided a vehicle comprising the all-solid-state battery as described herein.
[0028] Other aspects of the invention are discussed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The above and other features of the present invention will now be described in detail with reference to certain exemplary embodiments of the invention shown in the accompanying drawings, which are given hereinafter by way of illustration only, the present invention therefore not being limited to said drawings, and in which:
[0030] Figure 1 An exemplary all-solid-state battery according to an exemplary embodiment of the present invention is shown;
[0031] Figure 2 An exemplary coating according to an exemplary embodiment of the present invention is shown.
[0032] It should be understood that the drawings are not necessarily to scale, and represent various preferred features of the basic principles of the invention in a slightly simplified manner. The specific design features of the present invention disclosed herein, including, for example, specific size, orientation, location, and shape, will be determined in part by the specific intended application and use environment.
[0033] In the drawings, like reference numbers refer to the same or equivalent parts of the present invention throughout the several figures of the drawing. DETAILED DESCRIPTION
[0034] From the following description of the embodiments given with reference to the accompanying drawings, the above-mentioned objects, other objects, advantages and features of the present invention will become apparent. However, the present invention is not limited to the embodiments disclosed herein and can be implemented in various different forms. These embodiments are provided in order to fully describe the present invention and fully convey its scope to those skilled in the art.
[0035] In the following description of the embodiment, even in different drawings, the same element is represented by the same reference numeral. In the accompanying drawings, in order to make the description clearer, the size of the structure may be exaggerated compared to its actual size. In the following description of the embodiment, terms such as "first" and "second" can be used to describe various elements, but are not limited to these elements. These terms are only used to distinguish an element from other elements. For example, without departing from the scope and spirit of the present invention, the first element can be named as the second element, and similarly, the second element can be named as the first element. Singular expressions can include plural expressions unless they have significantly different contextual meanings.
[0036] In the following description of the embodiments, terms such as "comprising", "including" and "having" should be interpreted as indicating the presence of the described features, numbers, steps, operations, elements or components, or combinations thereof, in the description; and do not exclude the presence of one or more other features, numbers, steps, operations, elements or components, or combinations thereof, or the possibility of increasing them. In addition, it should be understood that when a component, such as a layer, film, region or plate, is referred to as being "on" another component, the component can be located "directly on" the other component, or other components can be inserted between the two components. Similarly, it should be understood that when a component, such as a layer, film, region or plate, is referred to as being "below" another component, the component can be located "directly under" the other component, or other components can be inserted between the two components.
[0037] All numbers, values and / or expressions representing the amounts of components, reaction conditions, polymer compositions and mixtures used in this specification are approximate values, which reflect the various uncertainties in the measurements when obtaining these values from essentially different things. Therefore, unless otherwise specified, it should be understood that they are modified by the term "about". In addition, unless otherwise specified or obvious from the context, the term "about" used herein should be understood to be within a range of normal tolerance in the field, such as within 2 standard deviations of the mean. "About" can be understood to be within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05% or 0.01% of the value. Unless the context clearly stipulates otherwise, all numerical values provided herein are modified by the term "about".
[0038] In addition, it should be understood that if a numerical range is disclosed in the specification, unless otherwise stated, the range includes all continuous values from the minimum value of the range to the maximum value. In addition, if the range refers to an integer, unless otherwise stated, the range includes all integers from the minimum integer to the maximum integer. In this specification, when describing the range of a variable, it should be understood that the variable includes all values, including the endpoints within the range. For example, the range "5 to 10" should be understood to include any sub-range, such as 6 to 10, 7 to 10, 6 to 9, 7 to 9, etc., and a single value of 5, 6, 7, 8, 9 and 10, and it should also be understood to include any value between valid integers within the range, such as 5.5, 6.5, 7.5, 5.5 to 8.5, 6.5 to 9, etc. In addition, for example, the range "10% to 30%" should be understood to include sub-ranges such as 10% to 15%, 12% to 18%, 20% to 30%, etc., and all integers including values of 10%, 11%, 12%, 13%, etc. up to 30%, and should also be understood to include any values between the valid integers in the said range, such as 10.5%, 15.5%, 25.5%, etc.
[0039] It should be understood that the term "vehicle" or "vehicle" or other similar terms used herein generally include motor vehicles, such as passenger cars including sport utility vehicles (SUVs), buses, trucks, various commercial vehicles, water vehicles including various boats and ships, aircraft, etc., and include hybrid vehicles, electric vehicles, plug-in hybrid electric vehicles, hydrogen-powered vehicles and other alternative fuel vehicles (e.g., fuels derived from resources other than petroleum). As described herein, a hybrid vehicle is a vehicle with two or more power sources, such as gasoline power and electric power.
[0040] Figure 1 An exemplary all-solid-state battery 100 according to an exemplary embodiment of the present invention is shown. The all-solid-state battery 100 may include an anode 10, a cathode 20, and a solid electrolyte layer 30 between the anode 10 and the cathode 20. Each component will be described in detail below.
[0041] negative electrode
[0042] The negative electrode 10 may include a negative electrode current collector 11 , a coating layer 12 disposed on the negative electrode current collector, and a negative electrode layer 13 disposed on the coating layer 12 and including a negative electrode material.
[0043] The negative electrode current collector 11 may preferably be a plate-shaped base material having conductivity. For example, the negative electrode current collector 11 may be in the form of a sheet, a film, or a foil.
[0044] The negative electrode current collector 11 may include a material that does not react with lithium. Preferably, the negative electrode current collector 11 may appropriately include nickel (Ni), copper (Cu), stainless steel, or a combination thereof.
[0045] The thickness of the negative electrode current collector 11 is not limited to a specific value, and may be, for example, about 1 μm to 500 μm.
[0046] Figure 2 An exemplary coating layer 12 according to an exemplary embodiment of the present invention is shown. The coating layer 12 may include pores formed by entanglement of the metal nanowires 123. The coating layer 12 may include a mesh structure in which the metal nanowires 123 are entangled.
[0047] The coating layer 12 may be formed by randomly entangled metal nanowires 123 and thus has a large specific surface area and excellent electrical conductivity.
[0048] The coating layer 12 may include a first layer 121 configured to be in contact with the negative electrode current collector 11 and including pores.
[0049] The specific surface area of the first layer 121 increases, thereby increasing the contact area with the negative electrode collector 11 and having excellent bonding strength with the negative electrode collector 11. Therefore, the content of the binder in the negative electrode layer 13 can be reduced, the resistance in the negative electrode 10 can be reduced, and the detachment of the negative electrode active material 13 caused by the volume expansion of the silicon-based negative electrode active material in the negative electrode active material 13 can be prevented.
[0050] The coating layer 12 may include a second layer 122 material disposed on the first layer 121 and configured so that the pores are filled with a portion of the negative electrode material 124 of the negative electrode layer 13. The negative electrode material 124 may include a silicon-based negative active material 124a, a solid electrolyte 124b, and the like.
[0051] Since the metal nanowires 123 and the negative electrode material 124 are mixed in the second layer 122, the second layer 122 can improve the conductivity of the negative electrode 10. Therefore, the content of the conductive material in the negative electrode layer 13 can be reduced, and the resistance of the negative electrode 10 can be reduced.
[0052] The metal nanowires 123 may appropriately include nickel (Ni), copper (Cu), or a combination thereof.
[0053] The metal nanowire 123 may have a length of about 5 μm to 25 μm and a diameter of about 10 nm to 50 nm. The diameter of the metal nanowire 123 may mean the diameter of the cross section of the metal nanowire 123 when the metal nanowire 123 is cut in a direction perpendicular to the length direction of the metal nanowire 123. When the length of the metal nanowire 123 is less than about 5 μm, the coating layer 12 may have difficulty in maintaining its structure; and when the length of the metal nanowire 123 is greater than about 25 μm, the metal nanowires may aggregate, the specific surface area of the second layer 122 may be reduced, and pores may not be formed, and therefore, the second layer 122 may not be filled with the negative electrode material 124.
[0054] The negative electrode layer 13 may include a negative electrode material.
[0055] The negative electrode material may include a silicon-based negative electrode active material, a solid electrolyte, a conductive material, a binder, and the like.
[0056] Silicon-based negative electrode active materials may include Si, SiO x (0<x<2) or a combination thereof. In addition, the silicon-based negative electrode active material may further include a carbonaceous material. For example, the silicon-based negative electrode active material may be obtained by coating a carbonaceous material on a core material including a silicon compound, or may be obtained by coating a silicon compound on a core material including a carbonaceous material.
[0057] The solid electrolyte may include a sulfide-based solid electrolyte. The sulfide-based solid electrolyte may include Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (m and n are positive numbers and Z is one of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (x and y are positive numbers and M is one of P, Si, Ge, B, Al, Ga and In), Li 10 G 2 S 12 wait.
[0058] The conductive material may include carbon black, conductive graphite, ethylene black, graphene, and the like.
[0059] The adhesive may include styrene butadiene rubber, nitrile rubber, butadiene rubber, polyvinylidene fluoride, polytetrafluoroethylene, and the like.
[0060] The thickness of the negative electrode layer 13 may be greater than the thickness of the second layer 122. When the thickness of the negative electrode layer 13 is less than the thickness of the second layer 122, the metal nanowires 123 of the second layer 122 may penetrate the negative electrode layer 13 and the solid electrolyte layer 30, so that a short circuit may occur, and the content of the negative electrode material in the negative electrode 10 may decrease, so that the energy density and capacity of the negative electrode 10 may decrease.
[0061] Specifically, the thickness of the negative electrode layer 13 may be about 25 μm to 30 μm. The thickness of the first layer 121 may be about 6 μm to 10 μm. The thickness of the second layer 122 may be about 5 μm to 10 μm.
[0062] The method of manufacturing the negative electrode 10 may include the following steps: preparing a solution including a precursor of the metal nanowires 123; obtaining an intermediate by coating the solution on the negative electrode collector 11; obtaining a coating layer 12 including pores formed by forming the metal nanowires on the negative electrode collector 11 by heat-treating the intermediate; and forming a negative electrode layer by coating a slurry including a negative electrode material on the coating layer 12. The metal nanowires 123 may be heat-treated to form an entangled state.
[0063] The precursor of the metal nanowire 123 may include an oxide or sulfide of nickel, copper, etc. The precursor of the metal nanowire 123 may include NiC 2 O 4 、NiSO 4 ,CuC 2 O 4 ,CuSO 4 wait.
[0064] The solution may be prepared by dissolving the precursor of the metal nanowires 123 in a solvent such as acid, water, or the like.
[0065] The solution can be alkaline. For example, the pH of the solution can be greater than about 7 but equal to or less than about 14. 3 NH 4 OH etc. can make it alkaline.
[0066] The solution may also include a reducing agent. The reducing agent may include N 2 H 4 wait.
[0067] The intermediate may be obtained by coating the solution on the negative electrode current collector 11. The coating of the solution is not limited to a specific method, and may be performed using a spin coating method, a spray coating method, a deep coating method, or the like.
[0068] Thereafter, the precursor of the metal nanowires 123 may be reduced by heat-treating the intermediate to form the coating layer 12 .
[0069] In particular, the coating layer 12 may be formed by heat-treating the intermediate at a temperature equal to or higher than about 120° C. but lower than about 140° C. When the heat treatment temperature is lower than 120° C., the precursor cannot be reduced, and thus the metal nanowires 123 may not be formed, and when the heat treatment temperature is equal to or higher than 140° C., the metal nanowires 123 may aggregate, and thus the coating layer 12 may not adhere to the negative electrode current collector 11.
[0070] In addition, the coating layer 12 may be formed by heat-treating the intermediate for more than about 10 hours but equal to or less than about 12 hours. When the heat treatment time is equal to or less than 10 hours, the reduction amount of the precursor is insufficient, and thus the coating layer 12 may not be properly formed; when the heat treatment time is greater than 12 hours, the reduction amount of the precursor is too large, and metal nanoparticles other than the metal nanowires 123 may be formed.
[0071] Thereafter, the pores in the coating layer 12 may be filled with part of the negative electrode material, and the negative electrode layer 13 may be formed on the coating layer 12 by applying a slurry including the negative electrode material to the coating layer 12 .
[0072] Finally, the negative electrode 10 may be manufactured by drying the negative electrode current collector 11 , the coating layer 12 , and the negative electrode layer 13 .
[0073] positive electrode
[0074] The positive electrode 20 may include a positive electrode collector 21 and a positive electrode active material layer 22 disposed on the positive electrode collector.
[0075] The positive electrode current collector 21 may include a plate-shaped substrate having conductivity. The positive electrode current collector 21 may include an aluminum foil.
[0076] The thickness of the positive electrode current collector 21 is not limited to a specific value, and may be, for example, about 1 μm to 500 μm.
[0077] The positive electrode active material layer 22 may include a positive electrode active material, a solid electrolyte, a conductive material, a binder, and the like.
[0078] The positive electrode active material can store and release lithium ions.
[0079] The positive electrode active material may include a rock salt layer-type active material such as LiCoO 2 、LiMnO 2 、LiNiO 2 、LiVO 2 or Li 1+x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ; Spinel-type active material, such as LiMn 2 O 4 Or Li(Ni 0.5 Mn 1.5 ) 4; Inverted spinel-type active materials, such as LiNiVO 4 or LiCoVO 4 ; Olivine-type active materials, such as LiFePO 4 、LiMnPO 4 、LiCoPO 4 or LiNiPO 4 ; Silicon-containing active materials, such as Li 2 FeSiO 4 or Li 2 MnSiO 4 ; Rock salt layer-type active materials in which a part of the transition metals are replaced by another metal, such as LiNi 0.8 Co (0.2-x) Al x O 2 (0 < x < 0.2); Spinel-type active materials in which a part of the transition metals are replaced by another metal, such as Li 1+x Mn 2-x-y M y O 4 (M is at least one of Al, Mg, Co, Fe, Ni or Zn, and 0 < x + y < 2), or lithium titanate, such as Li 4 Ti 5 O 12 .
[0080] The solid electrolyte may include an oxide-based solid electrolyte or a sulfide-based solid electrolyte.
[0081] The oxide-based solid electrolyte may include perovskite-type LLTO (Li 3x La 2 / 3-x TiO 3 ), phosphate-based NASICON-type LATP (Li 1+x Al x Ti 2-x (PO 4 ) 3 ), etc.
[0082] The sulfide-based solid electrolyte may include Li 2 S-P 2 S 5 、Li 2 S-P 2 S 5 -LiI、Li 2 S-P 2 S 5 -LiCl、Li 2 S-P 2 S5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (m and n are positive numbers and Z is one of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (x and y are positive numbers, M is one of P, Si, Ge, B, Al, Ga and In), Li 10 G 2 S 12 wait.
[0083] The conductive material may include carbon black, conductive graphite, ethylene black, graphene, etc. The conductive material included in the positive electrode active material layer 22 may be the same as or different from the conductive material included in the negative electrode layer 13 .
[0084] The binder may include butadiene rubber, nitrile rubber, hydrogenated nitrile rubber, polyvinylidene fluoride, polytetrafluoroethylene, etc. The binder included in the positive active material layer 22 may be the same as or different from the binder included in the negative electrode layer 13 .
[0085] Solid electrolyte layer
[0086] The solid electrolyte layer 30 may be interposed between the negative electrode 10 and the positive electrode 20 , and may include a solid electrolyte having lithium ion conductivity.
[0087] The solid electrolyte may include an oxide-based solid electrolyte or a sulfide-based solid electrolyte.
[0088] Oxide-based solid electrolytes may include perovskite-type LLTO (Li 3x La 2 / 3-x TiO 3 ), phosphate-based NASICON-type LATP (Li 1+x Al x Ti 2-x (PO 4 ) 3 )wait.
[0089] Sulfide-based solid electrolytes may include Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (m and n are positive numbers and Z is one of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (x and y are positive numbers, M is one of P, Si, Ge, B, Al, Ga and In), Li 10 G 2 S 12 wait.
[0090] The solid electrolyte included in the solid electrolyte layer 30 may be the same as or different from the solid electrolyte included in the positive electrode active material layer 22 . Example
[0091] Hereinafter, the present invention will be described in more detail by the following examples. The following examples are only used to exemplarily describe the present invention and are not intended to limit the scope of the present invention.
[0092] Example 1
[0093] By using NiSO as a precursor of metal nanowires 4 Dissolve in water, inject sodium hydroxide (NaOH) into it to adjust the pH of the solution to greater than 7, and then inject N as a reducing agent into it. 2 H 4 to prepare the solution.
[0094] An intermediate was obtained by coating the solution on a nickel foil used as a negative electrode current collector.
[0095] The intermediate was heat-treated at 120° C. for 11 hours to reduce the precursor, thereby obtaining a coating layer including pores formed by entanglement of metal nanowires.
[0096] The negative electrode active material and the solid electrolyte are placed in a planetary disperser (PD) mixer and dry mixed. A slurry is obtained by adding a binder, a dispersant and a solvent to the resulting product and mixing them. The slurry is applied to the coating using a scraper and then dried at a temperature of about 90°C to form a negative electrode layer.
[0097] The negative electrode was manufactured by vacuum drying a stack including the negative electrode current collector, the coating layer and the negative electrode layer at a temperature of about 120° C. for about 4 hours.
[0098] Example 2
[0099] A negative electrode was manufactured in the same manner as in Example 1, except that the intermediate was heat-treated for 12 hours.
[0100] Example 3
[0101] A negative electrode was manufactured in the same manner as in Example 1, except that the intermediate was heat-treated at a temperature of 130°C.
[0102] Example 4
[0103] A negative electrode was manufactured in the same manner as in Example 1, except that the intermediate was heat-treated at a temperature of 130° C. for 12 hours.
[0104] Comparative Example
[0105] A negative electrode excluding a coating layer was manufactured. A negative electrode layer was prepared by directly coating the slurry of Example 1 on a nickel foil used as a negative electrode current collector and then drying the slurry at a temperature of about 90°C.
[0106] The negative electrode was manufactured by vacuum drying a stack including the negative electrode current collector, the coating layer and the negative electrode layer at a temperature of about 120° C. for about 4 hours.
[0107] The adhesive strength and resistance of the negative electrodes of Examples 1 to 4 and Comparative Example were evaluated. The evaluation results are shown in Table 1 below.
[0108] The adhesive strength of each negative electrode according to Examples 1 to 4 refers to the adhesive strength between the coating layer and the negative electrode collector, and the adhesive strength of the negative electrode according to the comparative example refers to the adhesive strength between the negative electrode layer and the negative electrode collector.
[0109] The adhesive strength of each negative electrode was measured by the following method using a 180° peel strength tester. - Preparation of test specimens: A piece of specimen with a size of 25 mm x 150 mm was cut from each negative electrode and adhered to a slide glass (25 mm x 75 mm). - Test: Each specimen in which only half of the negative electrode is adhered to the slide glass is fixed to the lower end of the tester and turned 180 degrees. The negative electrode is fixed to the upper end of the tester and pulled at a speed of 30 mm / min, and the value of the applied force is measured. - Results: The average bond strength was calculated by dividing the force (grams-force) applied on a cross section of 20 mm to 40 mm by the width (ie 25 mm).
[0110] The resistance of each negative electrode was measured using an electrode resistance measurement system. The electrode resistance measurement system is a device that calculates resistance based on a voltage value measured when a sample is placed on a measurement component with a probe and then current is applied to the measurement component. The measurement conditions are as follows. <Measurement conditions> -Current: 10mA - Voltage range: within 0.5V Table 1
[0111] As shown in the above Table 1, it can be confirmed that the resistance of the negative electrode including the coating according to Examples 1 to 4 is much lower than that of the negative electrode according to the comparative example. In addition, the negative electrodes according to Examples 1 and 2 are excellent in bonding strength compared to the negative electrode according to the comparative example. Therefore, when the coating including pores formed by entanglement of metal nanowires according to various exemplary embodiments of the present invention is inserted between the negative electrode current collector and the negative electrode layer, the resistance of the negative electrode can be reduced and the bonding strength between the layers can be increased.
[0112] As is apparent from the above description, according to the present invention, there can be provided a negative electrode for an all-solid-state battery having excellent bonding strength between a negative electrode layer and a negative electrode collector and a method for manufacturing the same.
[0113] According to the present invention, a negative electrode for an all-solid-state battery having excellent conductivity and a method for manufacturing the same can be provided.
[0114] The present invention has been described in detail with reference to its exemplary embodiments. However, it will be appreciated by those skilled in the art that these embodiments may be modified without departing from the principles and spirit of the invention, the scope of the invention being defined by the appended claims and their equivalents.
Claims
1. A negative electrode for an all-solid-state battery, include: Anode current collector; a coating layer, the coating layer i) being disposed on the negative electrode current collector and ii) comprising pores formed by metal nanowires; and a negative electrode layer, the negative electrode layer being disposed on the coating layer and comprising a negative electrode material, wherein the coating comprises a mesh structure in which the metal nanowires are entangled, The coating comprises: a first layer, the first layer being configured to contact the negative electrode current collector; and A second layer is provided on the first layer and is configured so that the pores are filled with at least a portion of the negative electrode material of the negative electrode layer. 2 . The negative electrode according to claim 1 , wherein the metal nanowires comprise nickel (Ni), copper (Cu), or a combination thereof. 3 . The negative electrode according to claim 1 , wherein the metal nanowire has a length of about 5 μm to 25 μm and a diameter of about 10 nm to 50 nm. The negative electrode according to claim 1 , wherein a thickness of the negative electrode layer is greater than a thickness of the second layer. 5 . The negative electrode according to claim 1 , wherein the negative electrode layer has a thickness of about 25 μm to 30 μm. The negative electrode according to claim 1 , wherein the first layer has a thickness of about 6 μm to 10 μm. The negative electrode according to claim 1 , wherein the second layer has a thickness of about 5 μm to 10 μm. 8 . The negative electrode according to claim 1 , wherein the negative electrode material comprises a silicon-based negative electrode active material and a solid electrolyte.
9. A method for manufacturing a negative electrode for an all-solid-state battery, wherein include: preparing a solution containing a precursor of metal nanowires; Obtaining an intermediate by coating the solution on a negative electrode current collector; obtaining a coating layer including pores formed by forming metal nanowires on the negative electrode current collector by heat-treating the intermediate; and forming a negative electrode layer by applying a slurry including a negative electrode material onto the coating layer, The coating comprises: a first layer, the first layer being configured to contact the negative electrode current collector; and A second layer is provided on the first layer and is configured so that the pores are filled with at least a portion of the negative electrode material of the negative electrode layer.
10. The method of claim 9, wherein the solution is alkaline.
11. The method of claim 9, wherein the solution further comprises a reducing agent.
12. The method according to claim 9, in, In obtaining the coating, the intermediate is heat treated at a temperature equal to or higher than about 120°C but lower than about 140°C.
13. The method according to claim 9, in, In obtaining the coating, the intermediate is heat treated for a period of time greater than about 10 hours but equal to or less than about 12 hours.
14. The method of claim 9, wherein the metal nanowires comprise nickel (Ni), copper (Cu), or a combination thereof. 15 . The method of claim 9 , wherein the metal nanowire has a length of about 5 μm to 25 μm and a diameter of about 10 nm to 50 nm.
16. The method according to claim 9, in, The thickness of the negative electrode layer is greater than the thickness of the second layer. 17 . The method according to claim 9 , wherein the thickness of the negative electrode layer is about 25 μm to 30 μm.
18. The method of claim 9, wherein the first layer has a thickness of about 6 μm to 10 μm. The method of claim 9 , wherein the second layer has a thickness of about 5 μm to 10 μm. 20 . The method according to claim 9 , wherein the negative electrode material comprises a silicon-based negative electrode active material and a solid electrolyte.