Non-aqueous electrolyte and lithium ion battery

By using nonaqueous electrolyte in lithium-ion batteries, combining compounds A and B, the high impedance problem caused by electrolyte additives is solved, and the fast charging and high-low temperature performance of lithium-ion batteries are improved, which significantly improves the battery overall performance.

CN119069810AActive Publication Date: 2024-12-03HEFEI SMOOTHWAY ELECTRONIC MATERIALS CO LTD +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411491560.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-03
Estimated Expiration
2044-10-24

Smart Images

  • Figure CN119069810A_ABST
    Figure CN119069810A_ABST
Patent Text Reader

Abstract

The invention discloses a non-aqueous electrolyte and a lithium ion battery, the non-aqueous electrolyte comprises a lithium salt, an organic solvent and an additive, the organic solvent comprises a carbonic ester compound, the additive comprises a compound A and a compound B, the structure of the compound A is shown as a formula 1, and the structure of the compound B is shown as a formula 2; in the imgabs0 #, R1 and R2 are respectively and independently selected from C1-C6 alkyl, halogen and C1-C6 halogen substituted alkyl; and R3 is selected from C1-C6 alkyl groups, C2-C6 alkenyl groups, C2-C6 alkynyl groups and cyano groups. According to the non-aqueous electrolyte disclosed by the invention, the compound A and the compound B are combined, so that the impedance of the battery can be reduced, and the fast charging capacity and high and low temperature performance of the lithium ion battery are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a non-aqueous electrolyte and a lithium ion battery. Background Art

[0002] Since the commercialization of lithium-ion batteries, they have been widely used in various fields of daily life and production due to their advantages such as high energy density, excellent cycle life and low self-discharge rate. Lithium-ion batteries are not only an important cornerstone for promoting the development of the new energy industry, but also play a vital role in many industries such as electricity, transportation, industry, communications, construction and military, supporting the widespread application of new energy technologies. With the development of these specific application fields, the requirements for the high and low temperature performance, storage performance and fast charging capability of lithium-ion batteries are also increasing.

[0003] The electrolyte plays a vital role in lithium-ion batteries. It is the medium for lithium ions to be transferred between the positive electrode and the negative electrode. The electrochemical performance of lithium-ion batteries is largely related to the electrode / electrolyte interface characteristics. In the prior art, additives are usually introduced into the electrolyte to adjust the chemical composition and properties of the electrode / electrolyte interface, thereby improving the electrochemical performance of the battery. However, most of the current additives usually exhibit high impedance in lithium-ion batteries, resulting in the inability to simultaneously take into account the battery's fast charging capability and high and low temperature performance.

[0004] Therefore, there is an urgent need to develop a non-aqueous electrolyte to reduce the impedance of the battery itself, so that the lithium-ion battery can have both fast charging capability and high and low temperature performance. Summary of the invention

[0005] In view of the above problems, the object of the present invention is to provide a non-aqueous electrolyte and a lithium-ion battery, which can reduce the impedance of the battery and significantly improve the fast charging capability and high and low temperature performance of the lithium-ion battery.

[0006] To achieve the above objectives, the first aspect of the present invention provides a non-aqueous electrolyte, comprising a lithium salt, an organic solvent and an additive, wherein the organic solvent comprises a carbonate compound, and the additive comprises a compound A and a compound B, wherein the structure of the compound A is shown in Formula 1 below, and the structure of the compound B is shown in Formula 2 below;

[0007]

[0008] Wherein R1 and R2 are each independently selected from C1-C6 alkyl, halogen, C1-C6 halogen-substituted alkyl; R3 is selected from C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, cyano (-C≡N) 。

[0009] Compound A has good oxidation resistance, so the introduction of compound A in non-aqueous electrolyte can make lithium-ion batteries less likely to produce gas at high temperature and high voltage. However, in practical applications, the presence of compound A will deteriorate the fast charging ability of lithium-ion batteries, resulting in a decrease in charging rate, thereby limiting the widespread use of lithium-ion batteries in application scenarios that require fast charging. Compound B has a relatively low oxidation potential and can be oxidized on the electrode surface before the solvent to form a thinner interface layer. The interface layer has a better lithium ion transmission efficiency, which helps to reduce the impedance of the battery and improve the fast charging ability and low temperature performance of the lithium-ion battery; in addition, compound B contains alkoxy groups, so the alkoxy-containing interface formed by compound B is easily dissolved in carbonate solvents, causing the battery interface to be unstable, resulting in the deterioration of the high temperature characteristics of the battery. The inventor of the present application found in the process of invention that the alkoxy-containing interface formed by compound B is not easily dissolved in carbonate solvents when compound A is introduced into carbonate solvents, which is conducive to the protective characteristics of the alkoxy interface on the electrode material, so that the high temperature performance of lithium-ion batteries at high voltage is significantly improved. Therefore, the non-aqueous electrolyte of the present invention combines compound A and compound B, which can reduce the impedance of the battery and significantly improve the fast charging capability and high and low temperature performance of the lithium-ion battery.

[0010] Further, the C1-C6 alkyl group of the present invention may be, but is not limited to, methyl, ethyl, propyl, butyl, pentyl, and hexyl; the halogen may be fluorine (F), chlorine (Cl), bromine (Br), and iodine (I); the C1-C6 halogen-substituted alkyl group may be, but is not limited to, monofluoromethyl (-CH2F), difluoromethyl (-CHF2), trifluoromethyl (-CF3), 1,1-dichloroethyl (-CHCl2), 2,2,2-trifluoroethyl (-CH2CF3), 2-chloropropyl (-CH2CHClCH3), 3-chloropropyl (-CH2CH2CH2Cl), and 1,1,1-trifluorobutyl (-CH2CH2CH2CF3); the C2-C6 alkenyl group may be, but is not limited to, vinyl (-C2H3), propenyl (-C3H5), butenyl (-C4H7), pentenyl (-C5H9), hexenyl (-C6H 11 ); C2~C6 alkynyl may be, but is not limited to, ethynyl (-C≡CH), propynyl (-CH2C≡CH), butynyl (-C4H5), pentynyl (-C5H7), hexynyl (-C6H9).

[0011] Furthermore, the compound A of the present invention is at least one selected from the group consisting of compounds A1 to A3:

[0012]

[0013] Furthermore, the compound B of the present invention is selected from at least one of compounds B1 to B4:

[0014]

[0015] Specifically, the side chains of compound B2 and compound B3 contain unsaturated bonds, which can undergo polymerization reaction on the surface of the negative electrode to improve the toughness of the negative electrode interface, thereby further improving the low-temperature performance of the lithium-ion battery.

[0016] Further, the mass percentage of compound A of the present invention in the non-aqueous electrolyte is 0.1-10%. Specifically, the mass percentage of compound A in the non-aqueous electrolyte may be, but is not limited to, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 7%, 8%, 9%, 10%.

[0017] Further, the mass percentage of the compound B of the present invention in the non-aqueous electrolyte is 0.1-10%. Specifically, the mass percentage of the compound B in the non-aqueous electrolyte may be, but is not limited to, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%.

[0018] Further, the lithium salt of the present invention includes at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate, lithium tetrafluoroborate (LiBF4), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide, lithium methanesulfonate, lithium trifluoromethylsulfonate, lithium fluorosulfonate, lithium bis(oxalate)borate, lithium difluorooxalate borate, lithium difluorophosphate, lithium difluorobis(oxalate)phosphate, lithium diphosphate and lithium lower aliphatic carboxylate. Specifically, the mass percentage of the lithium salt in the non-aqueous electrolyte is 5 to 30%, such as the content of the lithium salt can be but not limited to 5%, 10%, 15%, 20%, 25%, 30%; preferably, the mass percentage of the lithium salt in the non-aqueous electrolyte is 5 to 18%.

[0019] Further, the carbonate compounds of the present invention include cyclic carbonates and chain carbonates. Specifically, the cyclic carbonates may be, but are not limited to, ethylene carbonate, propylene carbonate, butylene carbonate, pentylene carbonate, vinylene carbonate or their derivatives; chain carbonates include, but are not limited to, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate.

[0020] Further, the organic solvent of the present invention also includes at least one of a carboxylate compound and an ether compound. By mixing carboxylate compounds, ether compounds and carbonate compounds, the comprehensive performance of the electrolyte can be further improved. For example, carboxylate compounds can provide a higher dielectric constant, ether compounds can provide better low-temperature performance, and carbonate compounds can provide better film-forming properties.

[0021] Furthermore, the carboxylic acid esters of the present invention include at least one of cyclic carboxylic acid esters and chain carboxylic acid esters. The cyclic carboxylic acid esters may specifically include but are not limited to at least one of γ-butyrolactone, γ-valerolactone, and δ-valerolactone; the chain carboxylic acid esters include but are not limited to methyl acetate, ethyl acetate, propyl acetate, butyl acetate, propyl propionate, and butyl propionate.

[0022] Furthermore, the ether compounds of the present invention include cyclic ethers or chain ethers. The cyclic ethers may specifically include but are not limited to at least one of 1,3-dioxolane (DOL), 1,4-dioxolane (DX), crown ethers, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH3-THF), and 2-trifluoromethyltetrahydrofuran (2-CF3-THF); the chain ethers may specifically include but are not limited to dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether.

[0023] Furthermore, the non-aqueous electrolyte of the present invention further comprises an auxiliary agent, which is selected from vinylene carbonate (VC), vinylene carbonate (VEC), fluoroethylene carbonate (FEC), vinyl sulfite (ES), 1,3-propane sultone (PS), 1,3-propylene sultone (PES), 1,4-butane sultone (BS), vinyl sulfate (DTD), succinic anhydride (SA), maleic anhydride (MA), 2-methylmaleic anhydride (MMA), methyl carbonate-2-propynyl ester, tetravinylsilane, triallyl At least one of isocyanurate, hexamethylene diisocyanate, o-phenanthroline, p-phenylene diisocyanate, 2,4-toluene diisocyanate, N-phenyl bis(trifluoromethanesulfonyl)imide, vinyl disulfate, phenyl methanesulfonate, vinyl disulfate, bis-spiro-propylene sulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, isocyanoethyl methacrylate, methylene disulfonate, tri(trimethylsilyl)borate, tri(trimethylsilyl)phosphate, and tri(vinyldimethylsilyl)phosphate. Specifically, the mass percentage of the auxiliary agent of the present invention in the non-aqueous electrolyte is 0.1-5%, such as the auxiliary agent content can be but not limited to 0.1%, 0.5%, 1%, 1.6%, 1.9%, 2.6%, 3.2%, 3.8%, 4.3%, 4.8%, and 5%. Preferably, the mass percentage of the auxiliary agent in the non-aqueous electrolyte is 0.1-2%.

[0024] Accordingly, the second aspect of the present invention further provides a lithium ion battery, comprising a positive electrode, a negative electrode, and the above-mentioned non-aqueous electrolyte. The lithium ion battery has low impedance and good fast charging capability and high and low temperature performance.

[0025] Furthermore, the active materials of the positive electrode of the present invention include lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. Specifically, the lithium-containing phosphates with an olivine structure include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. Lithium transition metal oxides include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (structure such as LiNi x Co y Mn 1-x-y M z O2, wherein 0.6≤x<0.9, x+y<1, 0≤z<0.08, M is at least one of Al, Mg, Zr and Ti). Preferably, the active material of the positive electrode of the present invention is LiNi 0.8 Co 0.1 Mn 0.1 Zr 0.03 O2.

[0026] Furthermore, the active material of the negative electrode of the present invention includes at least one of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, and a lithium negative electrode. The carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, mesophase carbon microspheres, etc.; the silicon-based negative electrode may include silicon materials, silicon oxides, silicon-carbon composite materials, and silicon alloy materials, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, and tin metal compounds; the lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium silicon alloy, a lithium sodium alloy, a lithium potassium alloy, a lithium aluminum alloy, a lithium tin alloy, and a lithium indium alloy. DETAILED DESCRIPTION

[0027] In order to further illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific examples. It should be noted that, if specific conditions are not specified in the examples and comparative examples, they can be carried out according to conventional conditions or conditions recommended by the manufacturer, and if the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0028] Example 1

[0029] This embodiment provides a method for preparing a lithium ion battery, the steps comprising:

[0030] (1) The ternary material LiNi 0.8 Co 0.1 Mn 0.1 Zr 0.03O2, conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 96.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector. The coating amount is 324g / m 2 , dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and then dried at 85°C for 4 hours under vacuum conditions, and the tabs were welded to make positive electrode sheets that meet the requirements;

[0031] (2) artificial graphite and silicon are mixed in a mass ratio of 90:10, and then mixed with a conductive agent SuperP, a thickener CMC, and an adhesive SBR (styrene-butadiene rubber latex) in a mass ratio of 95:1.5:1.0:2.5 to make a slurry, which is mixed evenly, and the mixed slurry is applied on both sides of a copper foil, and then dried and rolled to obtain a negative electrode sheet, thereby making a negative electrode sheet that meets the requirements;

[0032] (3) In a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethyl propionate (EP), and propyl propionate (PP) are mixed in a mass ratio of 2:2:5:2:1 to obtain a mixed solvent as an organic solvent, and then additives and auxiliary agents are added to obtain a mixed solution. The mixed solution is sealed and packaged and placed in a quick freezer (-4°C) for 2 hours, then taken out, and in a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), lithium hexafluorophosphate is slowly added to the mixed solution, and a non-aqueous electrolyte is obtained after mixing evenly;

[0033] (4) The positive electrode sheet, negative electrode sheet and separator are laminated to form a lithium-ion battery with a thickness of 4.7 mm, a width of 55 mm and a length of 60 mm. The battery is vacuum-baked at 75°C for 10 h and the non-aqueous electrolyte is injected. After standing for 24 h, the battery is charged to 4.4 V at a constant current of 0.1 C (180 mA), and then charged at a constant voltage of 4.4 V until the current drops to 0.05 C (90 mA); then discharged to 3.0 V at 0.2 C (180 mA), and the charge and discharge are repeated twice. Finally, the battery is charged to 3.8 V at 0.2 C (180 mA) to obtain a lithium-ion battery.

[0034] The formulations of the non-aqueous electrolytes of Examples 1 to 17 and Comparative Examples 1 to 6 are shown in Table 1, wherein the preparation processes of the non-aqueous electrolytes, positive electrode sheets, negative electrode sheets, and lithium-ion batteries of Examples 2 to 17 and Comparative Examples 1 to 6 are the same as those of Example 1.

[0035] Table 1 Formula of non-aqueous electrolyte of Examples and Comparative Examples

[0036]

[0037]

[0038] The following performance tests were performed on the lithium ions prepared in Examples 1 to 17 and Comparative Examples 1 to 6. The test results are shown in Table 2.

[0039] Impedance test:

[0040] The impedance of the battery after capacity division was tested by an electrochemical workstation with a frequency range of 0.01 to 10 Hz to obtain the total impedance value of the lithium-ion battery.

[0041] High temperature storage performance test :

[0042] At room temperature (25°C), the lithium-ion battery was charged and discharged at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.4V, and then the battery was charged to 4.4V under 0.5C constant current and constant voltage conditions, and the battery thickness was measured (the thickness was recorded as D0); the battery was placed in a 60°C oven for 30 days, taken out and the battery thickness was measured (the thickness was recorded as D1); the battery was placed in a 25°C environment and discharged at 0.5C (the discharge capacity was recorded as C1); the lithium-ion battery was continued to be charged and discharged at room temperature (25°C) at 0.5C / 0.5C (the battery discharge capacity was recorded as C2), with an upper limit voltage of 4.4V, and the capacity retention rate, capacity recovery rate and thickness expansion rate were calculated.

[0043] Capacity retention rate = (C1 / C0)*100%

[0044] Capacity recovery rate = (C2 / C0)*100%

[0045] Thickness expansion rate = (D1 / D0)*100%

[0046] Normal temperature cycle performance test :

[0047] At room temperature (25°C), the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 1.0C / 1.0C for 500 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.

[0048] Capacity retention rate = (C1 / C0)*100%

[0049] High temperature cycle performance test :

[0050] Under high temperature (45°C) conditions, the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 1.0C / 1.0C for 400 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.

[0051] Capacity retention rate = (C1 / C0)*100%

[0052] Low temperature performance test :

[0053] At room temperature (25°C), the lithium-ion battery is charged and discharged at 0.5C / 0.5 (battery cut-off voltage is 3.0V, discharge capacity is C0), and the upper limit voltage is 4.4V (cut-off current 0.05C). Then the battery is fully charged to 4.4V (cut-off current 0.05C) at 0.5C at room temperature (25°C), and then the battery is transferred to -20°C and left for 4 hours, and discharged to 3.0V at 0.5C, and the discharge capacity is C1. The capacity retention rate is calculated.

[0054] Capacity retention rate = (C1 / C0)*100%

[0055] Rate performance test:

[0056] The lithium-ion battery is charged and discharged for 5 cycles at a 5C rate at room temperature, and the 5C capacity retention rate is obtained = the discharge capacity in the fifth cycle / the 1C discharge capacity at room temperature.

[0057] Table 2 Performance test results of lithium ion batteries of the embodiments and comparative examples

[0058]

[0059]

[0060] As can be seen from Table 2, compared with Comparative Example 1, Examples 1 to 17, because their non-aqueous electrolytes include Compound A and Compound B, have lithium-ion batteries that not only have good high-temperature storage and high-temperature cycle performance, but also have good low-temperature performance at -20°C, and also have good fast-charging performance. This is because Compound A can make lithium-ion batteries less likely to produce gas at high temperatures and high voltages, and Compound B helps to reduce the impedance of the battery and improve the fast-charging capability and low-temperature performance of lithium-ion batteries; importantly, the alkoxy-containing interface formed by Compound B is not easily dissolved in carbonate solvents containing Compound A, which is conducive to the protective properties of the alkoxy interface on the electrode material; therefore, the non-aqueous electrolyte of the present invention combines Compound A and Compound B, which can reduce the impedance of the battery and significantly improve the fast-charging capability and high and low-temperature performance of the lithium-ion battery.

[0061] By comparing Example 10 with Examples 11 to 14, it can be seen that adding auxiliary agents on the basis of the additives of the present invention can further improve the high temperature storage performance, high temperature cycle performance, low temperature performance of the lithium ion battery, and the lithium ion cycle performance is better and the expansion rate is lower.

[0062] By comparing Examples 15 to 17 with Examples 11 to 12, it can be seen that when VC / FEC mixed additives are used in the electrolyte, the high temperature performance and low temperature performance of the lithium ion battery are greatly improved, and the expansion rate is further improved.

[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A non-aqueous electrolyte comprising a lithium salt, an organic solvent and an additive, characterized in that: The organic solvent includes a carbonate compound, the additive includes a compound A and a compound B, the structure of the compound A is shown in Formula 1, and the structure of the compound B is shown in Formula 2; Wherein R1 and R2 are each independently selected from C1-C6 alkyl, halogen, C1-C6 halogen-substituted alkyl; R3 is selected from C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, and cyano.

2. The non-aqueous electrolyte according to claim 1, characterized in that The compound A is selected from at least one of compounds A1 to A3:

3. The non-aqueous electrolyte according to claim 1, characterized in that The compound B is selected from at least one of compounds B1 to B4:

4. The non-aqueous electrolyte according to claim 1, characterized in that The mass percentage of the compound A in the non-aqueous electrolyte is 0.1-10%.

5. The non-aqueous electrolyte according to claim 1, characterized in that The mass percentage of the compound B in the non-aqueous electrolyte is 0.1-10%.

6. The non-aqueous electrolyte according to claim 1, characterized in that The lithium salt includes at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethylsulfonyl imide), lithium methane sulfonate, lithium trifluoromethyl sulfonate, lithium fluorosulfonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobis(oxalatophosphate), lithium diphosphate and lithium lower aliphatic carboxylate.

7. The non-aqueous electrolyte according to claim 1, characterized in that The organic solvent further comprises at least one of a carboxylic acid ester compound and an ether compound.

8. The non-aqueous electrolyte according to claim 1, characterized in that It also includes an auxiliary agent, which is selected from vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate, succinic anhydride, maleic anhydride, 2-methylmaleic anhydride, methyl carbonate-2-propynyl ester, tetravinylsilane, triallyl isocyanurate, hexamethylene diisocyanate, o-phenanthroline, p-phenylene diisocyanate, 2, At least one of 4-toluene diisocyanate, N-phenylbis(trifluoromethanesulfonyl)imide, vinyl bissulfate, phenyl methanesulfonate, vinyl bissulfate, bis-spiro-propylene sulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, isocyanoethyl methacrylate, methylene disulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, and tris(vinyldimethylsilyl)phosphate.

9. A lithium ion battery comprising a positive electrode and a negative electrode, characterized in that: It also includes the non-aqueous electrolyte according to any one of claims 1 to 8.

10. The lithium ion battery according to claim 9, characterized in that The active material of the positive electrode includes olivine-structured lithium-containing phosphate, lithium transition metal oxide and their respective modified compounds.

Citation Information

Patent Citations

  • Lithium ion battery electrolyte solution and its additive

    CN103151560A

  • Electrolyte for improving high-temperature stability under high voltage and lithium secondary battery

    CN118782906A

  • Non-aqueous electrolyte and secondary battery

    WO2023179456A1

  • Non-aqueous electrolyte solution and secondary battery

    WO2024016897A1

  • Lithium-ion battery

    WO2024114176A1