Preparation method and application of MXene (at) MnO2 composite material for treating organic wastewater

The MXene@MnO2 composite material addresses the oxidation issue of MXene by forming a manganese dioxide coating, enhancing its stability and catalytic ozone oxidation performance for organic pollutant degradation.

CN119076032APending Publication Date: 2024-12-06SICHUAN UNIVERSITY OF SCIENCE AND ENGINEERING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411243066.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

MXene materials are easily oxidized in oxygen-rich environments, leading to reduced catalytic performance and stability, limiting their use in catalytic ozone oxidation for degrading organic pollutants.

Method used

A method is developed to prepare a MXene@MnO2 composite material by adding manganese salt to isopropanol solution, followed by titanium carbide dispersion and ultrasonic heating, then reacting with potassium permanganate to form manganese dioxide coating on the MXene surface, enhancing its stability and catalytic ozone oxidation capability.

Benefits of technology

The MXene@MnO2 composite material exhibits improved catalytic ozone oxidation degradation ability for organic pollutants, with enhanced stability and efficiency, achieving up to 99.8% degradation of specific pollutants compared to unmodified MXene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076032A_ABST
    Figure CN119076032A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an MXene (at) MnO2 composite material for treating organic wastewater, and the preparation method comprises the following steps: firstly, adding a certain amount of manganese salt into an isopropanol solution, then adding trititanium dioxide, carrying out ultrasonic dispersion, heating and stirring to obtain a suspension; dissolving potassium permanganate in water, and adding into the suspension; and finally, stirring at a constant temperature for a certain time, filtering, washing and drying to obtain the MXene (at) MnO2 composite material for treating organic wastewater. By compounding MnO2 and MXene, the ozone oxidation catalysis activity and stability of the MXene material can be improved, and the problem that the MXene material cannot be used for catalyzing ozone oxidation degradation of organic pollutants due to the fact that the MXene material is easy to oxidize in water is effectively solved; the catalyst has good catalytic ozonation degradation performance on chemical nickel plating wastewater, morpholine derivative organic wastewater, dye wastewater and antibiotic wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalytic ozone oxidation, and in particular to a preparation method and application of a MXene@MnO2 composite material for treating organic wastewater. Background Art

[0002] Catalytic ozone oxidation process is an advanced oxidation process (AOPs), which uses the strong oxidizing free radicals (such as hydroxyl free radicals, superoxide free radicals, etc.) generated during the reaction process to oxidize pollutants in water. In recent years, research has found that heterogeneous catalytic ozone oxidation process has the advantages of easy recycling, high activity and high cost performance compared with homogeneous process.

[0003] MXene material is a new type of two-dimensional transition metal carbide crystal material with the chemical formula of Mn+1Xn (n=1, 2 or 3, M is a transition metal element, and X is a carbon or nitrogen element). MXene material is considered to be a potential material due to its unique physical and chemical properties. Although compared with traditional nanomaterials, MXene has the advantages of large specific surface area, high hydrophilicity, abundant surface active sites and excellent chemical stability, these advantages make it have broad application prospects in the field of catalysis. However, it is easily oxidized in oxygen-rich environments such as air or water, resulting in its conversion into oxides, reduced catalytic performance and poor stability. Therefore, when using MXene materials as efficient catalysts, their stability needs to be modified. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a MXene@MnO2 composite material for treating organic wastewater and its application, which not only has the ability to efficiently catalyze ozone oxidation, but also improves some properties of the material itself, effectively solving the problem that MXene materials are easily oxidized in water and cannot be used for catalytic ozone oxidation to degrade organic pollutants.

[0005] To achieve the above object, the technical solution adopted by the present invention to solve the technical problem is: to provide a method for preparing a MXene@MnO2 composite material for treating organic wastewater, comprising the following steps:

[0006] S1, adding manganese salt to isopropanol solution, then adding titanium carbide, and heating and stirring after ultrasonic dispersion to obtain a suspension;

[0007] S2. Dissolve potassium permanganate in water, then add it dropwise to the suspension obtained in step S1, stir at a constant temperature, cool, filter, wash and dry to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0008] Further, in step S1, the manganese salt is one of manganese chloride, manganese sulfate, manganese nitrate and manganese carbonate.

[0009] Furthermore, in step S1, the mass volume ratio of the manganese salt and the isopropanol solution is 0.4-0.8 g:200 mL.

[0010] Furthermore, in step S1, the mass volume ratio of titanium carbide and isopropanol solution is 0.1-0.7 g:200 mL.

[0011] Furthermore, in step S1, the concentration of the isopropanol solution is 4-8 wt %.

[0012] Furthermore, in step S1, ultrasonic dispersion is performed for 1 to 3 hours, and the mixture is heated to 65 to 105° C. and stirred.

[0013] Further, in step S2, the mass volume ratio of potassium permanganate to water is 0.3-0.6 g:4-8 mL.

[0014] Furthermore, in step S2, the mixture is stirred at a constant temperature of 20 to 60° C. for 10 to 60 minutes and then cooled to room temperature.

[0015] Furthermore, in step S2, drying is performed under vacuum at 50 to 70° C. for 8 to 13 hours.

[0016] The MXene@MnO2 composite material for treating organic wastewater is prepared by the preparation method of the MXene@MnO2 composite material for treating organic wastewater.

[0017] The above-mentioned MXene@MnO2 composite material for treating organic wastewater is used in catalytic ozone oxidation treatment of chemical nickel plating wastewater, morpholine derivative organic wastewater, dye wastewater or antibiotic wastewater.

[0018] In summary, the present invention has the following beneficial effects:

[0019] 1. The MXene@MnO2 composite material prepared by the method provided by the present invention has good catalytic ozone ability, and the ozone oxidation degradation ability of Ni-EDTA wastewater, N-methylmorpholine wastewater, rhodamine b wastewater and tetracycline wastewater is improved by 99.8%, 93.1%, 94.2% and 88.5% respectively. Compared with the unmodified MXene material, it is not easy to be oxidized in water, and can be used for catalytic ozone oxidation degradation of organic pollutants in water for a longer time.

[0020] 2. The present invention first adds manganese salt to the isopropanol solution, which can not only make the titanium carbide added later dispersed evenly in the solution, but also make the divalent manganese uniformly loaded on the surface of titanium carbide. With manganese salt and potassium permanganate as manganese sources, potassium permanganate reacts with manganese salt on the surface of titanium carbide in water to form manganese dioxide, so that manganese dioxide is successfully coated on the surface of titanium carbide, so as to achieve the purpose that MXene is not easily oxidized in water. The experimental operation of the present invention is simple and feasible, and meets the requirements of green chemistry, energy conservation and emission reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The effect of different mass of titanium dicarbide on the catalytic performance of MXene@MnO2;

[0022] Figure 2 The effect of different heating time on the catalytic performance of MXene@MnO2;

[0023] Figure 3 The effects of different manganese salts on the catalytic performance of MXene@MnO2;

[0024] Figure 4 The effects of different solvents on the catalytic performance of MXene@MnO2;

[0025] Figure 5 The effects of different raw materials on the catalytic performance of MXene@MnO2;

[0026] Figure 6 The effect of different stirring times on the catalytic performance of MXene@MnO2;

[0027] Figure 7 The degradation ability of MXene@MnO2 catalyzed ozonation on different pollutants;

[0028] Figure 8 The comparison chart of XRD results of MXene and MXene@MnO2;

[0029] Fig. 9 This is the SEM image of MXene material (magnification 5μm);

[0030] Fig.10 This is the SEM image of MXene material (magnification 10 μm);

[0031] Fig.11 This is the SEM image of the MXene@MnO2 composite material prepared in Example 1 (magnification 500nm);

[0032] Fig.12 This is the SEM image of the MXene@MnO2 composite material prepared in Example 1 (magnification 5 μm). DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with the embodiments, but is not intended to limit the present invention.

[0034] Example 1

[0035] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0036] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0037] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0038] Example 2

[0039] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0040] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.7 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0041] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 4 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0042] Example 3

[0043] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0044] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.3 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0045] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 6 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0046] Example 4

[0047] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0048] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.1 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0049] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0050] Example 5

[0051] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0052] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 65° C. and stir to obtain a suspension;

[0053] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0054] Example 6

[0055] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0056] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 75° C. and stir to obtain a suspension;

[0057] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0058] Example 7

[0059] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0060] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 95° C. and stir to obtain a suspension;

[0061] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0062] Example 8

[0063] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0064] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 105° C. and stir to obtain a suspension;

[0065] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0066] Example 9

[0067] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0068] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0069] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 10 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0070] Example 10

[0071] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0072] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, heat to 85° C. and stir to obtain a suspension;

[0073] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 20 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0074] Embodiment 11

[0075] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0076] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, heat to 85° C. and stir to obtain a suspension;

[0077] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 40 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0078] Example 12

[0079] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0080] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, heat to 85° C. and stir to obtain a suspension;

[0081] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 50 min, cool to room temperature, remove the liquid, wash with deionized water 5 times, and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0082] Embodiment 13

[0083] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0084] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, heat to 85° C. and stir to obtain a suspension;

[0085] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 60 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0086] Embodiment 14

[0087] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0088] S1. Add 0.453 g of manganese sulfate to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0089] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0090] Embodiment 15

[0091] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0092] S1. Add 0.453 g of manganese nitrate to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0093] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0094] Example 16

[0095] A MXene@MnO2 composite material for treating organic wastewater, wherein the preparation method thereof comprises the following steps:

[0096] S1. Add 0.453 g of manganese carbonate to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0097] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times and vacuum dry at 60 ° C for 12 h to obtain a MXene@MnO2 composite material for treating organic wastewater.

[0098] Comparative Example 1

[0099] A MXene composite material, the preparation method of which comprises the following steps:

[0100] S1. Add 0.453 g of manganese chloride to 200 mL of pure water, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85 °C and stir to obtain a suspension;

[0101] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times, and vacuum dry at 60 ° C for 12 h to obtain a MXene composite material.

[0102] Comparative Example 2

[0103] A MXene composite material, the preparation method of which comprises the following steps:

[0104] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% acetone solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0105] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times, and vacuum dry at 60 ° C for 12 h to obtain a MXene composite material.

[0106] Comparative Example 3

[0107] A MXene composite material, the preparation method of which comprises the following steps:

[0108] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0109] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times, and vacuum dry at 60 ° C for 12 h to obtain a MXene composite material.

[0110] Comparative Example 4

[0111] A MXene composite material, the preparation method of which comprises the following steps:

[0112] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium aluminum carbide, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0113] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times, and vacuum dry at 60 ° C for 12 h to obtain a MXene composite material.

[0114] Comparative Example 5

[0115] A MXene composite material, the preparation method of which comprises the following steps:

[0116] S1. Add 0.453 g of manganese chloride to 200 mL of 5 wt% isopropanol solution, then add 0.5 g of titanium carbonitride, disperse by ultrasonic for 2 h, then heat to 85° C. and stir to obtain a suspension;

[0117] S2. Dissolve 0.379 g of potassium permanganate in 5 mL of water, then quickly add it to the suspension obtained in step S1, stir at a constant temperature for 30 min, cool to room temperature, remove the liquid, wash with deionized water 5 times, and vacuum dry at 60 ° C for 12 h to obtain a MXene composite material.

[0118] Test Example 1

[0119] In order to detect the catalytic performance of the MXene@MnO2 composite material, 0.2 g of the MXene@MnO2 prepared in Examples 1-16 and Comparative Examples 1-5 was added to 800 mL of Ni-EDTA solution (COD≈400 mg / L, Ni content≈58 mg / L), dispersed evenly by ultrasound, and then an ozone-oxygen mixture with a flow rate of 200 mL / min was introduced. After 45 minutes, the COD and Ni content of the solution were measured. 2+ The results are as follows Figure 1-Figure 5 As shown. Among them, Figure 1 0.1M, 0.3M, 0.5M, 0.7M and 0M are the experimental results of Example 4, Example 3, Example 1, Example 2 and a blank control group without adding MXene@MnO2, respectively; Figure 2 65T, 75T, 85T, 95T and 105T are the experimental results of Example 5, Example 6, Example 1, Example 7 and Example 8 respectively; Figure 3 , manganese chloride, manganese sulfate, manganese nitrate and manganese carbonate are the experimental results of Example 1, Example 14, Example 15 and Example 16 respectively; Figure 4 In, isopropanol, pure water and acetone are the experimental results of Example 1, Comparative Example 1 and Comparative Example 2 respectively; Figure 5 , Ti3C2, Ti2C, Ti3AlC2 and Ti3CN are the experimental results of Example 1, Comparative Example 3, Comparative Example 4 and Comparative Example 5 respectively; Figure 6 , 10min, 20min, 30min, 40min, 50min and 60min are the experimental results of Example 9, Example 10, Example 1, Example 11, Example 12 and Example 13 respectively.

[0120] Depend on Figure 1 It can be seen that compared with the blank control group 0M, the catalyst with added titanium carbide has the ability to catalyze ozone oxidation, and the optimal addition amount of titanium carbide is 0.5g. Too much or too little titanium carbide may cause uneven coating of manganese dioxide. When the addition amount is 0.5M, the removal rate of complex nickel is 99.8%, the COD removal rate is 97%, and the total nickel concentration is 0.08mg / L.

[0121] Depend on Figure 2It can be seen that since the boiling point of isopropanol is 82.3℃, it will be difficult for isopropanol to evaporate completely if the temperature is lower than this temperature, and too high a temperature will accelerate the oxidation of titanium dicarbide in water, both of which will affect the catalytic performance of the composite material. Therefore, 85℃ is a more suitable reaction temperature, with a removal rate of 99.8% for complex nickel, a removal rate of 97% for COD, and a total nickel concentration of 0.07mg / L.

[0122] Depend on Figure 3 It can be seen that MXene@MnO2 prepared with manganese chloride as manganese salt has stronger catalytic activity than manganese sulfate, manganese nitrate and manganese carbonate. The removal rate of complex nickel is 99.9%, the COD removal rate is 97%, and the total nickel concentration is 0.06 mg / L.

[0123] Depend on Figure 4 It can be seen that pure water environment will cause the MXene material to oxidize, resulting in a significant reduction in catalytic ability, and acetone's ability to disperse titanium dicarbide is not as good as that of isopropanol solution. The removal rate of complex nickel is 99.8%, the COD removal rate is 97%, and the total nickel concentration is 0.08 mg / L.

[0124] Depend on Figure 5 It can be seen that compared with other MXene materials, trititanium carbide is more suitable for catalytic ozone system. The removal rate of complex nickel is 99.8%, the COD removal rate is 97%, and the total nickel concentration is 0.08 mg / L.

[0125] Depend on Figure 6 It can be seen that too short a stirring time will lead to insufficient evaporation of isopropanol, while too long a stirring time will make titanium carbide more easily oxidized. Therefore, 30 minutes is a suitable stirring time. The removal rate of complex nickel is 99.8%, the COD removal rate is 97%, and the total nickel concentration is 0.08 mg / L.

[0126] Test Example 2

[0127] In order to detect the catalytic performance of the MXene@MnO2 composite material, 0.2 g of the MXene@MnO2 prepared in Example 1 was added to 800 mL of N-methylmorpholine wastewater, rhodamine b wastewater and tetracycline wastewater, respectively, and dispersed evenly by ultrasonication. Then, an ozone-oxygen mixture with a flow rate of 200 mL / min was introduced. After 45 minutes, the COD of the solution was measured by sampling. The results are shown in FIG. Figure 7 shown.

[0128] Depend on Figure 7 It can be seen that the MXene@MnO2 catalytic ozonation prepared in Example 1 has excellent degradation efficiency for different types of organic pollutants, and the COD removal rates are 93.1%, 94.2% and 88.5%, respectively.

[0129] Test Example 3

[0130] X-ray single crystal diffractometer was used to characterize MXene and MXene@MnO2 prepared in Example 1. Figure 8 shown.

[0131] Depend on Figure 8 It can be seen that the peak of Mn-MXene is reduced and more chaotic than the characteristic peak of MXene due to the coating of MnO2, which shows that the method provided in Example 1 can successfully coat manganese dioxide.

[0132] Test Example 4

[0133] The MXene@MnO2 prepared in Example 1 was characterized by scanning electron microscopy, and the obtained SEM image is as follows: Figure 9-12 shown.

[0134] Depend on Figure 9-12 It can be seen that MXene material is a multilayered catalytic material, and the solution of Example 1 successfully coats manganese dioxide on the surface of MXene to form a composite material.

[0135] Test Example 5

[0136] Take 0.25 g of the MXene@MnO2 composite material prepared in Example 1 as the adsorbent, add 1 L of Ni 2+ The simulated wastewater with a concentration of 77 mg / L was slowly stirred and adsorbed for 4 hours. After the adsorption, the solution was filtered through a filter membrane and Ni was detected 2+ When the concentration is 0.05 mg / L, the adsorption capacity can reach 307 mg / g.

[0137] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a MXene@MnO2 composite material for treating organic wastewater, characterized in that: The following steps are involved: S1, adding manganese salt to isopropanol solution, then adding titanium carbide, and heating and stirring after ultrasonic dispersion to obtain a suspension; S2. Dissolve potassium permanganate in water, then add it dropwise to the suspension obtained in step S1, stir at a constant temperature, cool, filter, wash and dry to obtain a MXene@MnO2 composite material for treating organic wastewater.

2. The method for preparing the MXene@MnO2 composite material for treating organic wastewater according to claim 1, characterized in that: In step S1, the manganese salt is one of manganese chloride, manganese sulfate, manganese nitrate and manganese carbonate.

3. The method for preparing the MXene@MnO2 composite material for treating organic wastewater according to claim 1, characterized in that: In step S1, the mass volume ratio of the manganese salt to the isopropanol solution is 0.4-0.8 g:200 mL; the mass volume ratio of the titanium carbide to the isopropanol solution is 0.1-0.7 g:200 mL.

4. The method for preparing the MXene@MnO2 composite material for treating organic wastewater according to claim 1, characterized in that: In step S1, the concentration of the isopropanol solution is 4-8 wt%.

5. The method for preparing the MXene@MnO2 composite material for treating organic wastewater according to claim 1, characterized in that: In step S1, ultrasonic dispersion is performed for 1 to 3 hours, and the mixture is heated to 65 to 105° C. and then stirred.

6. The method for preparing the MXene@MnO2 composite material for treating organic wastewater according to claim 1, characterized in that: In step S2, the mass volume ratio of potassium permanganate to water is 0.3-0.6 g:4-8 mL.

7. The method for preparing a MXene@MnO2 composite material for treating organic wastewater according to claim 1, characterized in that: In step S2, the mixture is stirred at a constant temperature of 20 to 60°C for 10 to 60 minutes and then cooled to room temperature.

8. The method for preparing the MXene@MnO2 composite material for treating organic wastewater according to claim 1, characterized in that: In step S2, drying is performed under vacuum at 50 to 70° C. for 8 to 13 hours.

9. A MXene@MnO2 composite material for treating organic wastewater prepared by the preparation method of a MXene@MnO2 composite material for treating organic wastewater according to any one of claims 1 to 8.

10. The MXene@MnO2 composite material for treating organic wastewater according to claim 9 is used in catalytic ozone oxidation treatment of chemical nickel plating wastewater, morpholine derivative organic wastewater, dye wastewater or antibiotic wastewater.