ZnCuInSexS2-x or ZnSnyCuInS2 quantum dot, composition and preparation method of ZnCuInSexS2 quantum dot

The ZnCuInSexS2-x or ZnSnyCuInS2 five-membered quantum dots were prepared by thermal injection method, and the optical band gap was regulated, which solved the problem of optical band gap width of existing quantum dots and improved the efficiency of solar cells.

CN119080054APending Publication Date: 2024-12-06ORDOS INST OF APPLIED TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028163.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing quantum dot optical band gap is wide, which limits the ability to capture sunlight and cannot meet the requirements of light capture efficiency, electron injection efficiency and charge collection efficiency at the same time.

Method used

The thermal injection method is used to prepare ZnCuInSexS2-x or ZnSnyCuInS2 five-membered quantum dots. By adjusting the ratio of Se/S or Sn/S ion mixture, the optical band gap of the quantum dots is regulated, the band gap is reduced to 2.41 eV, and the light absorption range and light absorption are improved. strength.

Benefits of technology

The band gap narrowing of quantum dots is achieved, the photoelectric performance of solar cells is improved, and the efficiency of solar cells is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2W5NXG9KBAAD2OCLGDQA25QOLVJYNKEJPOGTAHOD
    Figure 2W5NXG9KBAAD2OCLGDQA25QOLVJYNKEJPOGTAHOD
  • Figure 6NUM05HXPYJQHZJFF6MEGQBKVCCCQTZN4TFGML4G
    Figure 6NUM05HXPYJQHZJFF6MEGQBKVCCCQTZN4TFGML4G
  • Figure 8RFVUQNKWA7BAIYCQS4HVFBEDIA81OCUFWWVGSMD
    Figure 8RFVUQNKWA7BAIYCQS4HVFBEDIA81OCUFWWVGSMD
Patent Text Reader

Abstract

The invention discloses a ZnCuInSexS2-x or ZnSnyCuInS2 quantum dot, a composition and a preparation method of the ZnCuInSexS2 or ZnSnyCuInS2 quantum dot, and belongs to the technical field of quantum dots. The preparation method of the ZnCuInSexS2-x or ZnSnyCuInS2 quantum dot comprises the following steps: mixing a Zn source precursor solution, In (OAc) 3, CuI, oleylamine and octadecene, vacuumizing and heating to 55-65 DEG C, injecting a Se / S ion mixture or a Sn / S ion mixture to react when the temperature is raised to 160-170 DEG C, then cooling to 80-90 DEG C, and adding petroleum ether to obtain the ZnCuInSexS2-x quantum dot or the ZnSnyCuInS2 quantum dot. The invention also comprises the quantum dot prepared by the preparation method. The invention further provides a composition which comprises the two quantum dots. The quantum dot prepared by the preparation method is narrow in band gap.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of quantum dot technology, and in particular to a ZnCuInSe x S 2-x or ZnSn y CuInS2 quantum dots, compositions and preparation methods thereof. Background Art

[0002] From the primitive society of slash-and-burn farming to the current industrial society with rapid economic development, the daily per capita energy consumption has experienced exponential growth. With the rapid growth of global energy consumption, these non-renewable energy sources cannot be effectively compensated, and the world is facing severe problems such as energy depletion, environmental pollution and global warming. Therefore, the development of sustainable energy (such as solar energy, wind energy, hydropower and tidal energy, etc.) is imminent. Compared with wind energy and hydropower, solar energy has the advantages of large reserves, convenient access and not easily affected by the geographical environment. Researchers have found that the solar energy absorbed by the earth's surface in one hour can be used by humans all over the world for one year. Therefore, how to reasonably and efficiently develop and utilize solar energy is very important for the future development of mankind. The technology of converting solar energy into electricity, heat energy, fuel gas and biomass energy has been widely developed and utilized. Although the current prospects of solar energy are broad, its high cost and low efficiency have brought great challenges to the large-scale application of solar energy. Therefore, how to design a low-cost system that can effectively collect, transmit and store solar energy has become one of the most eye-catching issues.

[0003] According to the evolution of efficiency and cost, solar cells have gone through three generations of development: the first generation is inorganic solid-state batteries represented by single crystal, polycrystalline and amorphous silicon solar cells. The first generation of solar cells has entered the market due to its advantages of high efficiency and good stability, but the raw materials for preparing silicon cells are expensive, harmful substances are generated during the production process, and the energy conversion efficiency has tended to the theoretical value. These shortcomings limit the development of the first generation of solar cells. The second generation of solar cells is called thin-film solar cells. The manufacture of thin-film solar cells can use different technologies, such as vapor deposition, electrochemical deposition, magnetron sputtering and printing, which are much simpler than the manufacturing process and cost of the first generation of solar cells. However, due to its high content of toxic elements, low conversion efficiency and high cost, the second generation of solar cells has developed slowly. The third generation of solar cells is a sensitized solar cell based on emerging photovoltaic technology. This type of cell has the advantages of high theoretical efficiency, simple preparation process, and green environmental protection. The third generation of solar cells has attracted more attention from scientific researchers and is in a stage of rapid development.

[0004] Quantum dots have unique properties, such as quantum confinement effect, good visible light absorption, abundant surface active sites, multi-exciton effect, etc. This makes quantum dots one of the most attractive materials and is widely used in catalysis, sensing, solar cells, imaging and medicine. At present, quaternary quantum dots represented by ZnCuInS2 and ZnCuInSe2 have been widely studied by researchers. ZnCuInS2 has a higher conduction band edge than ZnCuInSe2, and photogenerated electrons have a stronger driving force to be injected into the photoanode. However, due to the large band gap, the absorption range is narrowed, which weakens the ability to capture sunlight. It can be seen that quantum dots with a single anion component or a single cation component cannot simultaneously meet the requirements of key performance aspects such as light capture efficiency, electron injection efficiency and charge collection efficiency. Summary of the invention

[0005] The purpose of the present invention is to overcome the above technical deficiencies and provide a ZnCuInSe x S 2-x or ZnSn y CuInS2 quantum dots, compositions and preparation methods thereof solve the technical problem of wide optical band gap of quantum dots in the prior art.

[0006] To address the above problems, we first used hot injection to prepare ZnCuInSe based on group I-III-VI quantum dots. x S 2-x Quinary quantum dots and ZnSn y CuInS2 quinary quantum dots.

[0007] In order to achieve the above technical purpose, the technical solution of the present invention provides a ZnCuInSe x S 2-x or ZnSn y The preparation method of CuInS2 quantum dots comprises the following steps: The Zn source precursor solution, In(OAc)3, CuI, oleylamine and octadecene ODE are mixed, vacuumed and heated to 55-65°C, then heated to 95-100°C in a nitrogen atmosphere and kept warm, then vacuumed again and the reaction system is heated in a nitrogen atmosphere, then heated to 160-170°C and Se / S ion mixture or Sn / S ion mixture is injected to react, then cooled to 80-90°C and petroleum ether is added to obtain ZnCuInSe x S 2-x Quantum dots or ZnSn y CuInS2 quantum dots.

[0008] In any embodiment, the Zn source precursor solution is prepared by the following steps: The Zn(OAc)2, octadecene and oleylamine are mixed and heated to 55-60°C and evacuated, and then heated to 120-130°C and nitrogen is continuously introduced for heating to obtain the Zn source precursor solution.

[0009] In any embodiment, the heating time at 120-130° C. with nitrogen is 5-8 min.

[0010] In any embodiment, the Se / S ion mixture or the Sn / S ion mixture is prepared by the following steps: Mix the S powder and oleylamine, heat to 55-60°C, evacuate, and then heat to 80-90°C, continuously introduce nitrogen and keep heating to obtain a S source precursor solution; Se powder, diphenylphosphine and oleylamine are mixed and heated in a water bath to obtain a Se source precursor solution; alternatively, SnCl4·5H2O and oleylamine are mixed, heated to 55-60°C for vacuum degassing, and then continued to heat to 120-130°C and continue to introduce nitrogen for heating for 5-10 minutes, and after being fully dissolved, vacuum degassing is performed to obtain a Sn source precursor solution; The S source precursor solution is mixed with the Se source precursor solution or the Sn source precursor solution to obtain the Se / S ion mixture or the Sn / S ion mixture.

[0011] In any embodiment, the concentration of S in the S source precursor solution is 1-1.2 mol / L; the concentration of Se or Sn in the Se source precursor solution or the Sn source precursor solution is 0.25-0.35 mol / L.

[0012] In any embodiment, the concentration of Zn in the Zn source precursor solution is 0.1-0.2 mol / L.

[0013] In any embodiment, the temperature is heated to 95-100°C and maintained for 3-10 minutes.

[0014] In any embodiment, the temperature is raised to 160-170° C. and the Se / S ion mixture or Sn / S ion mixture is injected for a reaction time of 15-20 minutes.

[0015] In addition, the present invention also proposes a ZnCuInSe x S 2-x or ZnSn y CuInS2 quantum dots are prepared by the above preparation method.

[0016] In any embodiment, the value of x is 0.4-1.6, and the value of y is 0.02-0.08.

[0017] The present invention also provides a quantum dot composition, including the above-mentioned ZnCuInSe x S 2-x Quantum dots and ZnSn y CuInS2 quantum dots, the ZnCuInSe x S 2-x Quantum dots and the ZnSn y The molar ratio of CuInS2 quantum dots is 1:(0.4-0.6); where x=0.8, y=0.08.

[0018] Compared with the prior art, the beneficial effects of the present invention include: the ZnCuInSe x S 2-x or ZnSn y The preparation method of CuInS2 quantum dots comprises the following steps: mixing a Zn source precursor solution, In(OAc)3, CuI, oleylamine and octadecene ODE, vacuumizing and heating to 55-65°C, then heating to 95-100°C in a nitrogen atmosphere and keeping the temperature, vacuumizing again and continuing to heat the reaction system in a nitrogen atmosphere, injecting a Se / S ion mixture or a Sn / S ion mixture to react when the temperature rises to 160-170°C, then cooling to 80-90°C and adding petroleum ether to obtain ZnCuInSe x S 2-x Quantum dots or ZnSn y CuInS2 quantum dots. The quantum dots prepared by the preparation method of the present invention have a narrow band gap, which can be as low as 2.41 eV. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The ZnCuInSe prepared in Example 1 of the present invention x S 2-x XRD pattern of quantum dots.

[0020] Figure 2 The ZnCuInSe prepared in Example 1 of the present invention 0 .8 S 1.2 TEM image of quantum dots.

[0021] Figure 3 The ZnCuInSe prepared in Example 1 of the present invention 0 .8 S 1.2 XPS image of quantum dots.

[0022] Figure 4 The ZnCuInSe prepared in Example 1 of the present invention x S 2-x PL spectrum of quantum dots.

[0023] Figure 5The ZnCuInSe prepared in Example 1 of the present invention x S 2-x UV-visible absorption spectrum of quantum dots.

[0024] Figure 6 The ZnCuInSe prepared in Example 1 of the present invention x S 2-x Quantum dot battery efficiency.

[0025] Figure 7 The ZnSn prepared in Example 2 of the present invention y XRD pattern of CuInS2 quantum dots.

[0026] Figure 8 The ZnSn prepared in Example 2 of the present invention 0.08 TEM image of CuInS2 quantum dots.

[0027] Fig. 9 The ZnSn prepared in Example 2 of the present invention 0.08 XPS image of CuInS2 quantum dots.

[0028] Fig.10 The ZnCuInSe prepared in Example 2 of the present invention x S 2-x PL spectrum of quantum dots.

[0029] Fig.11 The ZnCuInSe prepared in Example 2 of the present invention x S 2-x UV-visible absorption spectrum of quantum dots.

[0030] Fig.12 The ZnCuInSe prepared in Example 2 of the present invention x S 2-x Quantum dot battery efficiency. DETAILED DESCRIPTION

[0031] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The range defined in this way can be inclusive or exclusive of end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, wherein a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0032] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0033] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0034] This specific embodiment provides a ZnCuInSe x S 2-x or ZnSn y The preparation method of CuInS2 quantum dots comprises the following steps: The Zn source precursor solution, In(OAc)3, CuI, oleylamine OAM and octadecene ODE were mixed, vacuumed and heated to 55-65°C, then heated to 95-100°C in a nitrogen atmosphere and kept warm for 3-10 minutes, then vacuumed again and continued to heat the reaction system in a nitrogen atmosphere, then heated to 160-170°C and injected with Se / S ion mixture or Sn / S ion mixture to react for 15-20 minutes, then cooled to 80-90°C and added with petroleum ether to obtain ZnCuInSex S 2-x Quantum dots or ZnSn y CuInS2 quantum dots; the concentration of Zn in the Zn source precursor solution is 0.1-0.2 mol / L.

[0035] In some embodiments, the Zn source precursor solution is prepared by the following steps: The Zn(OAc)2, ODE and OAM are mixed and heated to 55-60°C and evacuated, and then heated to 120°C-130°C and nitrogen is continuously introduced and heated for 5-8 minutes to obtain the Zn source precursor solution.

[0036] In some embodiments, the Se / S ion mixture or the Sn / S ion mixture is prepared by the following steps: Mix the S powder and OAM and heat to 55-60°C and evacuate, then heat to 80-90°C, continue to introduce nitrogen and keep heating to obtain a S source precursor solution; Se powder, diphenylphosphine (i.e., DPP) and OAM are mixed and heated in a water bath to obtain a Se source precursor solution; alternatively, SnCl4·5H2O and OAM are mixed, heated to 55-60°C for vacuum degassing, and then continued to heat to 120-130°C and continue to introduce nitrogen for heating for 5-10 minutes, and after being fully dissolved, vacuum degassing is performed to obtain a Sn source precursor solution.

[0037] The S source precursor solution is mixed with the Se source precursor solution or the Sn source precursor solution to obtain the Se / S ion mixture or the Sn / S ion mixture; the concentration of S in the S source precursor solution is 1-1.2 mol / L, and the concentration of Se or Sn in the Se source precursor solution or the Sn source precursor solution is 0.25-0.35 mol / L.

[0038] This specific implementation also proposes a ZnCuInSe x S 2-x or ZnSn y CuInS2 quantum dots are prepared by the above preparation method, with x values ​​ranging from 0.4 to 1.6 and y values ​​ranging from 0.02 to 0.08.

[0039] This specific embodiment also provides a quantum dot composition, including the above-mentioned ZnCuInSe x S 2-x Quantum dots and ZnSn y CuInS2 quantum dots, the ZnCuInSe x S 2-x Quantum dots and the ZnSn yThe molar ratio of CuInS2 quantum dots is 1:(0.4-0.6); where x=0.8, y=0.08.

[0040] It should be noted that, in the present invention, oleylamine is abbreviated as OAM, and octadecene is abbreviated as ODE.

[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0042] In the present invention, reference is made to “some embodiments”, “this embodiment”, examples, etc., which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0043] If similar descriptions of "first / second" appear in the application documents, the following instructions are added. In the following description, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged in a specific order or sequence where permitted, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein.

[0044] In this embodiment, the term "and / or" is merely a description of the association relationship between associated objects, indicating that three relationships may exist. For example, object A and / or object B may represent three situations: object A exists alone, object A and object B exist at the same time, and object B exists alone.

[0045] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0046] This embodiment proposes a ZnCuInSe x S 2-x Quantum dots are prepared by the following steps: Preparation of Zn source precursor solution: Add 0.22 g of Zn(OAc)2, 0.8 mL of ODE, and 2 mL of OAM into a three-necked flask, heat from room temperature to 60°C and evacuate, heat from 60°C to 130°C and introduce nitrogen, continue heating at 130°C with nitrogen for 5 min, evacuate and degas after full dissolution, cool to room temperature, transfer to a penicillin bottle and seal for storage to obtain a 0.1 mol / L Zn source precursor solution.

[0047] Preparation of S source precursor solution: 0.32 g of S powder and 10 mL of OAM were placed in a three-necked flask, heated from room temperature to 60°C and vacuum degassed, then heated from 60°C to 90°C and introduced nitrogen, and heated at 90°C for 5 min with nitrogen introduced. After being fully dissolved, the solution was vacuum degassed, cooled to room temperature, transferred to a penicillin bottle, and sealed for storage to obtain a 1 mol / L S source precursor solution.

[0048] Preparation of Se source precursor solution: 0.2369 g of Se powder, 2 mL of DPP and 10 mL of OAM were added to a penicillin bottle and heated in a water bath at 50 °C to prepare a 0.25 mol / L Se source precursor solution.

[0049] Preparation of Se / S ion mixture: Sampling the prepared S source precursor solution and Se source precursor solution according to the Se / S molar ratio of 0.4:1.6, 0.8:1.2, 1.2:0.8, 1.6:0.4, putting them into a penicillin bottle and stirring for 10 minutes for later use; Synthesis of ZnCuInSe x S 2-x Quantum dots: 0.8 ml of Zn source precursor solution, 0.2 mmol of In(OAc)3, 0.14 mmol of CuI, 4 mL of OAM and 8 mL of ODE were added to a three-necked flask, vacuumed and heated to 60 ° C, then replaced with N2 atmosphere and heated to 100 ° C, kept at 100 ° C for 3 min to allow the cationic reagent to fully dissolve, and vacuumed again for 2 min to ensure that there were no impurities such as oxygen and water vapor in the reaction atmosphere. The reaction system was heated under N2 atmosphere, and a total of 1 mmol of Se / S ion mixture was injected when the temperature rose to 170 ° C. After 15 minutes of reaction, the heating was stopped, and 10 ml of petroleum ether was added after cooling to 90 ° C. The addition of petroleum ether can make the quantum dots evenly dispersed, avoid agglomeration, and further improve the efficiency of solar cells; cooled to room temperature, taken out, and centrifuged and purified to prepare ZnCuInSe x S 2-x Quantum dots, where x is 0.4, 0.8, 1.2 and 1.6, the corresponding quantum dots are ZnCuInSe 0.4 S 1.6, ZnCuInSe 0.8 S 1.2 , ZnCuInSe 1.2 S 0.8 and ZnCuInSe 1.6 S 0.4 .

[0050] from Figure 1 It can be seen that ZnCuInSe x S 2-x The diffraction peak of quantum dots is between chalcopyrite CuInS2 and CuInSe2, corresponding to PDF standard cards JCPDS No. 32-0339 and JCPDS No. 23-0209, respectively. This indicates that the prepared product is not a mixture of ZnCuInSe2 and ZnCuInS2, but a homogeneous single ZnCuInSe x S 2-x Five-element alloy quantum dots. The diffraction peaks of the four samples all correspond to the (112), (220), and (312) crystal planes of the chalcopyrite structure, and no diffraction peaks appear, indicating that changing the Se doping concentration does not cause changes in the crystal structure, and no binary impurity compounds such as ZnSe, ZnS, and CuS are formed. This confirms that the crystal structure of the quantum dots is independent of the Se and S composition ratio, that is, the single chalcopyrite structure is maintained within the entire composition range. As the Se doping concentration increases, it can be clearly observed that the diffraction peak shifts toward the small angle direction, tending to approach the position of the standard PDF card CuInSe2 (No. 23-0209), which is caused by Se replacing S.

[0051] like Figure 2 As shown, ZnCuInSe was obtained by TEM test. 0.8 S 1.2 Representative morphology and particle size distribution of quantum dots. Figure 2 As can be seen from (a) and (b), the Se-doped quantum dots are evenly dispersed in dichloromethane without agglomeration and have a single morphology, which indicates that Se doping does not change the structure of the quantum dots themselves, but enters the quantum dot lattice in the form of an alloy. This indirectly indicates that the prepared quantum dots are uniform and homogeneous ZnCuInSe 0.8 S 1.2 This is consistent with the XRD analysis results. Figure 2 (c) It can be seen that the particle size range is 2~7 nm, and most of them are distributed between 4~5 nm. Through software calculation, ZnCuInSe 0.8 S 1.2 The average size of the quantum dots is about 4.36 nm, which meets the deposition requirements on the photoanode. Figure 2(d) It can be seen that the lattice fringes of the TEM image are very clear, indicating that these quantum dots have high crystallinity. The spacing between adjacent crystal planes is 0.33 nm, corresponding to the (112) crystal plane of the chalcopyrite structure.

[0052] In order to further analyze the oxidation state, chemical composition and valence band energy of quantum dots, ZnCuInSe 0 .8 S 1.2 The quantum dot samples were subjected to XPS testing. Figure 3 (a) is the full spectrum of the sample. After correction with the C1s standard peak, the peaks of Zn 2p, Cu2p, In 3d, Se 3d and S 2p can be observed. The peaks of the five elements are not obvious in the full spectrum, which is caused by the low content of quantum dots. Figure 3 (b) is the XPS spectrum of Zn. The two orbital binding energy peaks of Zn 2p are 1045.8 eV and 1022.7 eV, respectively. The difference between the two peaks is 23.1 eV, which is consistent with the standard binding energy value of Zn, indicating that the valence state of Zn in the five-element alloy quantum dots is +2. Figure 3 (c) is the XPS spectrum of Cu. The energy level of Cu is split into two orbits, Cu 2p3 / 2 and Cu 2p1 / 2, with binding energies at 952.4 eV and 932.5 eV, respectively. The difference between the two peaks is 19.9 eV, which is completely consistent with the standard value of Cu 19.9 eV, indicating that the Cu element exists in the quantum dot in the form of +1 valence. Figure 3 In (d), the orbital binding energy of the In element is located at 451.9 eV and 444.3 e V, with a difference of 7.6 eV, which indicates that In has a +3 valence in the quantum dot. Figure 3 The binding energy of Se 3d in (e) is located at 54.3 eV, which indicates that Se exists in the QD with a valence of -2. Figure 3 (f) shows the energy spectrum peak of S 2p. After peak separation, it can be seen that the positions of the two orbital binding energies are 162.5 eV and 161.3 eV. The higher binding energy may be related to ZnCuInSe 0 .8 S 1.2 S in the quantum dot lattice 2 - Correspondingly, the lower binding energy may be due to the excessive S binding to the QD surface to form a thioether bond double layer ligand.

[0053] Figure 4 ZnCuInSe with different Se and S doping ratios x S 2-xPL spectrum of quantum dots. First, the optimal excitation wavelength was determined to be 360 ​​nm through the excitation spectrum test. It can be seen from the figure that the luminescence range covers most of the visible light band. When Se / S is 0.4:1.6, the best fluorescence intensity is shown. As the Se doping ratio increases, the overall luminescence intensity weakens, but it is not a strict linear relationship. When Se / S is 1.6:0.4, the luminescence intensity is almost negligible. This is because quantum dots may form internal defect states due to stacking faults, twins and site missing during nucleation and growth. The increase in Se content in quantum dots brings a higher defect state density. Electrons and holes may recombine in defect energy levels during relaxation. Since most defects have poor stability, the energy after recombination is released in the form of heat energy. The recombination in the defect energy level reduces the probability of band edge recombination, which ultimately leads to a decrease in the luminescence intensity of quantum dots. At the same time, it can be seen that when the Se doping ratio increases, the emission peak position shows a slight red shift trend as a whole. Qualitative analysis shows that the band gap of alloy quantum dots gradually decreases. This is because the introduction of Se increases the content of lower band gap components. The above results demonstrate that the luminescence intensity and luminescence position have strong component dependence, and the introduction of defect states may reduce the injection of photogenerated electrons into the photoanode.

[0054] Figure 5 The middle is ZnCuInSe with different Se and S doping ratios x S 2-x Quantum dot UV-visible absorption spectrum, the inset is the curve of (αhν)2 versus hν, and the intersection of the X-axis and the tangent is the optical band gap of quantum dots of different components. As can be seen from the figure, with the increase of Se doping ratio, the absorption band edge appears red shift, increasing from 550 nm to about 900 nm. This is because Se doping causes composition changes, which in turn reduces the band gap of alloy quantum dots, which is consistent with the results of PL spectrum analysis; at the same time, the increase in Se doping ratio makes the quantum dot light absorption stronger, which will greatly improve the utilization rate of sunlight by the photoanode and point out the direction for improving the photoelectric performance of quantum dot solar cells. As can be seen from the inset, when Se / S is 0.4:1.6, 0.8:1.2, 1.2:0.8, 1.6:0.4, the corresponding optical band gaps are 3.25 eV, 2.83 eV, 2.57 eV, and 2.41 eV, respectively. In summary, Se doping increases both the light absorption range and light absorption intensity, and composition changes can regulate the band gap range of quantum dots.

[0055] Table 1 ZnCuInSe prepared in Example 1 x S 2-x Photoelectric performance parameters of quantum dots Sample name Voc(mV) Jsc(mA / cm2) FF η(%) ZnCuInSe0.4S1.6 442.01 13.18 0.57 3.36 ZnCuInSe0.8S1.2 447.71 13.98 0.59 3.66 ZnCuInSe1.2S0.8 446.01 13.32 0.58 3.45 ZnCuInSe1.6S0.4 440.61 12.36 0.57 3.12 from Figure 6It can be seen that when Se / S is 0.8:1.2, the highest cell efficiency is obtained. It can be seen from Table 1 that the open circuit voltage and fill factor of each cell do not change significantly. The main factor causing the improvement of cell efficiency is the increase in short-circuit current density. Combined with the analysis of UV and PL, Se / S does not show the best optical performance when it is 0.8:1.2. This is because Se doping introduces more internal defect states, which affects the injection of photogenerated electrons into the photoanode, but at the same time broadens the light absorption range and enhances the light absorption intensity. By adjusting the Se and S doping ratio, the cell can achieve an ideal balance in key performance aspects such as energy level position, light absorption intensity, light absorption range and defect state density.

[0056] This embodiment proposes a ZnSn y CuInS2 quantum dots are prepared by the following steps: Preparation of Zn source precursor solution: Add 0.22 g of Zn(OAc)2, 0.8 mL of ODE and 2 mL of OAM into a three-necked flask, heat from room temperature to 60°C and evacuate, heat from 60°C to 130°C and introduce nitrogen, continue heating at 130°C with nitrogen for 5 min, evacuate and degas after full dissolution, cool to room temperature, transfer to a penicillin bottle and seal for storage to obtain a 0.1 mol / L Zn source precursor solution.

[0057] Preparation of S source precursor solution: 0.32 g of S powder and 10 mL of OAM were placed in a three-necked flask, heated from room temperature to 60°C and vacuum degassed, then heated from 60°C to 90°C and introduced nitrogen, and heated at 90°C for 5 min with nitrogen introduced. After being fully dissolved, the solution was vacuum degassed, cooled to room temperature, transferred to a penicillin bottle, and sealed for storage to obtain a 1 mol / L S source precursor solution.

[0058] Preparation of Sn source precursor solution: 0.1753 g of SnCl4·5H2O and 10 mL of OAM were added to a three-necked flask, heated from room temperature to 60°C for vacuum degassing, then heated from 60°C to 130°C and introduced nitrogen to ensure that the experimental environment was oxygen-free to prevent oxidation. Nitrogen was continuously introduced and heated at 130°C for 5 min. After being fully dissolved, vacuum degassing was performed. After cooling to room temperature, the solution was transferred to a penicillin bottle and sealed to obtain a 0.05 mol / L Sn source precursor solution.

[0059] Preparation of Sn / S ion mixture: sampling the prepared S source precursor solution and Sn source precursor solution according to the Sn / S molar ratio of 0.02:2, 0.04:2, 0.06:2, 0.08:2, putting them into a penicillin bottle and stirring for 10 min for later use; Synthesis of ZnSn yCuInS2 quantum dots: 0.8 ml of Zn source precursor solution, 0.2 mmol of In(OAc)3, 0.14 mmol of CuI, 4 mL of OAM and 8 mL of ODE were added to a three-necked flask, vacuumed and heated to 60 °C, then replaced with N2 atmosphere and heated to 100 °C, kept at 100 °C for 3 min to allow the cationic reagent to fully dissolve, vacuumed again for 2 min to ensure that there were no impurities such as oxygen and water vapor in the reaction atmosphere, and the reaction system was heated under N2 atmosphere. When the temperature rose to 170 °C, a total of 1 mmol of Se / S ion mixture was injected. After 15 minutes of reaction, heating was stopped, and 10 ml of petroleum ether was added after the temperature dropped to 90 °C, the temperature was lowered, and centrifuged for purification and drying to prepare ZnSn y CuInS2 quantum dots, where y is 0.02, 0.04, 0.06 and 0.08, the corresponding quantum dots are ZnSn 0.02 CuInS2, ZnSn 0.04 CuInS2, ZnSn 0.06 CuInS2 and ZnSn 0.08 CuInS2.

[0060] 0.8 ml of Zn source precursor solution, 0.2 mmol of In(OAc)3, 0.14 mmol of CuI, 4 mL of OAM and 8 mL of ODE were added to a three-necked flask, vacuumed and heated to 60 ° C, then replaced with N2 atmosphere and heated to 100 ° C, kept at 100 ° C for 3 min to allow the cationic reagent to fully dissolve, and vacuumed again for 2 min to ensure that there were no impurities such as oxygen and water vapor in the reaction atmosphere. The reaction system was heated under N2 atmosphere, and a total of 1 mmol of Se / S ion mixture was injected when the temperature rose to 170 ° C. After 15 minutes of reaction, the heating was stopped, and 10 ml of petroleum ether was added after cooling to 90 ° C. The addition of petroleum ether can make the quantum dots evenly dispersed, avoid agglomeration, and further improve the efficiency of solar cells; after cooling to room temperature, it was taken out and centrifuged and purified to prepare ZnCuInSe x S 2-x Quantum dots, wherein x is 0.4, 0.8, 1.2 or 1.6.

[0061] from Figure 7 It can be seen that by comparing with the standard PDF card (No. 32-0339), the three characteristic peaks (27.875 ᵒ ,46.308 ᵒ and 54.793 ᵒ / 55.042 ᵒ) correspond to the (112), (204) and (312) / (116) crystal planes of the CuInS2 chalcopyrite structure, respectively, and the crystallinity is relatively good, which indicates that the five elements form a single crystal phase system, but because the quantum dot size is at the nanometer level, the half-peak width of the characteristic peak is relatively wide. Calculated by the Debye-Scherrer formula, the size of Zn and Sn co-doped CuInS2 quantum dots is about 4.8 nm. None of the three diffraction peaks show angular shifts, and no impurity peaks appear, which indicates that binary sulfides are not generated during the co-doping process of cations, but instead occupy copper ion vacancies and indium ion vacancies to form five-element alloy quantum dots.

[0062] Figure 8 For the synthesis of ZnSn 0 .08 TEM spectrum of CuInS2 quantum dots. Figure 8 As shown in (a) and (b), the spherical quantum dots are evenly distributed and well dispersed, proving that the co-doping of Zn and Sn quantum dots does not significantly change the crystal structure, nor does it affect the nucleation and growth process of the quantum dots. 0 .08 CuInS2 quantum dots have serious aggregation phenomenon, which makes it impossible for quantum dots to be deposited on the surface of the photoanode, while ZnSn 0 .08 CuInS2 quantum dots can be well dissolved in dichloromethane solvent, and the TEM spectrum also shows that the quantum dots are evenly dispersed, which shows that the introduction of Zn elements effectively balances the reaction activity of cations and promotes uniform nucleation of quantum dots. Through statistical calculations, the average size of quantum dots is 4.28 nm, and the particle size distribution area is mostly concentrated in the range of 4~6 nm. Figure 8 (e) The observed lattice fringe spacing is 0.303 nm, which is roughly consistent with the (112) crystal plane of the CuInS2 chalcopyrite structure. The clear lattice fringes indicate that the Zn and Sn co-doped quantum dots have good crystallinity. Figure 8 (f) is an electron diffraction pattern composed of three concentric rings, which correspond to the (112), (204) and (312) / (116) crystal planes from the inside to the outside. This result is consistent with the XRD analysis, which once again proves that the prepared ZnSn0 .08 CuInS2 quantum dots have a chalcopyrite tetragonal lattice structure.

[0063] The Zn and Sn co-doping strategy was used to balance the reactivity of the cationic precursors and prepare ZnSn with uniform size and easy dispersion in solvents. xCuInS2 quantum dots, PL spectrum proves that Zn and Sn co-doping mainly modifies the defects inside the quantum dot lattice. According to the analysis of UV data, changing the Sn doping amount can change the quantum dot band gap in the range of 2.74~2.90 eV, so that the energy level position of quantum dots and titanium oxide is more matched, and photogenerated electrons can be more effectively injected into the photoanode conduction band. x The CuInS2 quantum dot battery was subjected to JV testing, and it was determined that when the Sn doping amount was 0.08 mmol, the battery achieved a maximum efficiency of 3.78%. This was mainly due to the co-doping of Zn and Sn modifying the defects inside the quantum dot lattice, inhibiting the recombination of electron-hole pairs at the defect energy levels inside the lattice, and the appropriate doping ratio enabled the quantum dots and TiO2 to achieve the best energy level match.

[0064] XPS was used to study the ZnSn 0 .08 Surface composition and element oxidation states of CuInS2 quantum dots. Fig. 9 As shown in Figure 9 (b) and (c), the split peaks of Zn 2p are 1045.2 eV (2p1 / 2) and 1022.3 eV (2p3 / 2), with a difference of 22.9 eV, which proves that the Zn element is divalent; the split peaks of Sn 3d are located at 494.3 eV (2p3 / 2) and 485.9 eV (2p5 / 2), with a difference of 8.4 eV, which shows that the Sn element is tetravalent. Fig. 9 In (d), (e) and (f), the peaks of Cu 2p, In 3d and S 2p can prove that the valence states of the three elements Cu, In and S are positive monovalent, positive trivalent and negative divalent. Combined with XRD analysis, it can be inferred that the four cations of Zn, Sn, Cu and In quickly form bonds with the injection of sulfur source during the reaction, but Zn and Sn are more likely to form covalent bonds with S than In, and Zn and Sn are more likely to form covalent bonds with O than Cu. According to the principle of preferential orientation growth of quantum dots, Zn and Sn are likely to be located on the surface of quantum dots to eliminate the dangling bonds of S, and at the same time, some Zn and Sn are combined with O to prevent the quantum dots from being oxidized. Therefore, it is inferred that Zn and Sn co-doped quantum dots may exhibit stronger stability and better optical properties.

[0065] from Fig.10 It can be seen that there are two emission peaks located at around 460 nm and 725 nm respectively. Changing the doping amount does not cause the change of the emission peak position, and the original emission wavelength remains unchanged, which shows that ZnSn x The basic optical transition of CuInS2 quantum dots does not originate from surface defects, otherwise surface passivation will cause changes in the emission peak position. However, with the increase of doping amount, the emission peak intensity first decreases and then increases, so it is inferred that Zn and Sn co-doping mainly modifies the defects inside the quantum dot lattice.

[0066] Fig.11 It can be seen that the absorption range is about 400 to 750 nm. As the Sn doping amount increases, the absorption intensity gradually decreases, which may be caused by the size effect of the quantum dots. From the inset, it can be seen that the change in the Sn doping amount causes the band gap to change in the range of 2.74~2.90 eV, but the change in the band gap is not very obvious, which corresponds to the result that the luminescence position in the PL spectrum is not obvious.

[0067] Table 2 ZnCuInSe prepared in Example 2 x S 2-x Photoelectric performance parameters of quantum dots Sample name Voc(mV) Jsc(mA / cm2) FF η(%) ZnSn0.02CuInS2 446.27 13.37 0.58 3.46 ZnSn0.04CuInS2 443.16 11.91 0.57 3.03 ZnSn0.06CuInS2 440.72 12.92 0.57 3.27 ZnSn0.08CuInS2 447.38 14.44 0.58 3.78 The detailed photovoltaic performance parameters are listed in Table 2. From the data in the table, it can be seen that the fill factor has almost no change, and the improvement in battery efficiency mainly comes from the improvement of short-circuit current and open-circuit voltage. Fig.12 It can be seen that when the Sn doping amount increases from 0.02 mmol to 0.06 mmol, the battery efficiency first decreases and then increases, which is consistent with the change law of PL luminescence intensity, indicating that the main factor affecting the battery efficiency at this time is that Zn and Sn co-doping modify the defects inside the quantum dot lattice, inhibit the recombination of electron-hole pairs at the defect energy level inside the lattice, and inject more photogenerated electrons into the photoanode surface. When the Sn doping amount is 0.08 mmol, the battery achieves the highest efficiency of 3.78%.

[0068] This embodiment proposes a ZnCuInSe 0.8 S 1.2 Quantum dots are prepared by the following steps: Preparation of Zn source precursor solution: Add 0.22 g of Zn(OAc)2, 0.8 mL of ODE, and 2 mL of OAM into a three-necked flask, heat from room temperature to 55°C and evacuate, heat from 55°C to 125°C and introduce nitrogen, continue heating at 125°C with nitrogen for 8 min, evacuate and degas after full dissolution, cool to room temperature, transfer to a penicillin bottle and seal for storage to obtain a 0.1 mol / L Zn source precursor solution.

[0069] Preparation of S source precursor solution: 0.32 g of S powder and 10 mL of OAM were placed in a three-necked flask, heated from room temperature to 55°C and vacuum degassed, then heated from 55°C to 80°C and introduced nitrogen, and heated at 80°C for 5 min. After the solution was fully dissolved, it was vacuum degassed, cooled to room temperature, transferred to a penicillin bottle, and sealed to obtain a 1 mol / L S source precursor solution.

[0070] Preparation of Se source precursor solution: 0.2369 g of Se powder, 2 mL of DPP and 10 mL of OAM were added to a penicillin bottle and heated in a water bath at 50 °C to prepare a 0.25 mol / L Se source precursor solution.

[0071] Preparation of Se / S ion mixture: sampling the prepared S source precursor solution and Se source precursor solution according to the Se / S molar ratio of 0.8:1.2, putting them into a penicillin bottle and stirring for 10 minutes for later use; Synthesis of ZnCuInSe 0.8 S 1.2 Quantum dots: 0.8 ml of Zn source precursor solution, 0.2 mmol of In(OAc)3, 0.14 mmol of CuI, 4 mL of OAM and 8 mL of ODE were added to a three-necked flask, vacuumed and heated to 60°C, then replaced with N2 atmosphere and heated to 100°C. The flask was kept at 100°C for 3 min to allow the cationic reagent to fully dissolve. The flask was vacuumed again for 2 min to ensure that there were no impurities such as oxygen and water vapor in the reaction atmosphere. The reaction system was heated under N2 atmosphere. When the temperature rose to 170°C, a total of 1 mmol of Se / S ion mixture was injected. After 15 minutes of reaction, the heating was stopped, and 10 ml of petroleum ether was added after cooling to 90°C. The addition of petroleum ether can make the quantum dots evenly dispersed, avoid agglomeration, and further improve the efficiency of solar cells; ZnCuInSe was prepared after cooling to room temperature, centrifugation and purification. 0.8 S 1.2 Quantum dots.

[0072] This embodiment proposes a ZnSn y CuInS2 quantum dots are prepared by the following steps: Preparation of Zn source precursor solution: Add 0.22 g of Zn(OAc)2, 0.8 mL of ODE and 2 mL of OAM into a three-necked flask, heat from room temperature to 65°C and evacuate, heat from 65°C to 120°C and introduce nitrogen, continue heating at 120°C with nitrogen for 7 min, evacuate and degas after full dissolution, cool to room temperature, transfer to a penicillin bottle and seal for storage to obtain a 0.1 mol / L Zn source precursor solution.

[0073] Preparation of S source precursor solution: 0.32 g of S powder and 10 mL of OAM were placed in a three-necked flask, heated from room temperature to 60°C and vacuum degassed, then heated from 60°C to 85°C and introduced nitrogen, and heated at 85°C for 5 min with nitrogen introduced. After being fully dissolved, the solution was vacuum degassed, cooled to room temperature, transferred to a penicillin bottle, and sealed for storage to obtain a 1 mol / L S source precursor solution.

[0074] Preparation of Sn source precursor solution: 0.1753 g of SnCl4·5H2O and 10 mL of OAM were added to a three-necked flask, heated from room temperature to 55°C for vacuum degassing, then heated from 55°C to 125°C and introduced nitrogen to ensure that the experimental environment was oxygen-free to prevent oxidation. Nitrogen was continuously introduced and heated at 125°C for 10 min. After sufficient dissolution, vacuum degassing was performed. After cooling to room temperature, the solution was transferred to a penicillin bottle and sealed to obtain a 0.05 mol / L Sn source precursor solution.

[0075] Preparation of Sn / S ion mixture: sampling the prepared S source precursor solution and Sn source precursor solution according to the Sn / S molar ratio of 0.08:2, putting them into a penicillin bottle and stirring for 10 minutes for later use; Synthesis of ZnSn 0.08 CuInS2 quantum dots: 0.8 ml of Zn source precursor solution, 0.2 mmol of In(OAc)3, 0.14 mmol of CuI, 4 mL of OAM and 8 mL of ODE were added to a three-necked flask, vacuumed and heated to 55 °C, then replaced with N2 atmosphere and heated to 95 °C, kept at 95 °C for 6 min to allow the cationic reagent to fully dissolve, vacuumed again for 2 min to ensure that there were no impurities such as oxygen and water vapor in the reaction atmosphere, and the reaction system was heated under N2 atmosphere. When the temperature rose to 160 °C, a total of 1 mmol of Sn / S ion mixture was injected. After 20 minutes of reaction, heating was stopped, and 10 ml of petroleum ether was added after the temperature dropped to 80 °C, and the temperature was cooled, centrifuged, purified and dried to prepare ZnSn 0.08 CuInS2 quantum dots.

[0076] This embodiment provides a quantum dot composition, including ZnCuInSe prepared in embodiment 1 x S 2-x Quantum dots and ZnSn prepared in Example 2 y CuInS2 quantum dots, the ZnCuInSe x S 2-x Quantum dots and the ZnSn y The molar ratio of CuInS2 quantum dots is 1:0.4; wherein x=0.8, y=0.08; and the quantum dot composition is obtained by mixing two quantum dots.

[0077] This embodiment provides a quantum dot composition, including ZnCuInSe prepared in embodiment 1 x S 2-x Quantum dots and ZnSn prepared in Example 2 y CuInS2 quantum dots, the ZnCuInSe x S 2-x Quantum dots and the ZnSn yThe molar ratio of CuInS2 quantum dots is 1:0.5; wherein x=0.8, y=0.08; the quantum dot composition is obtained by mixing two quantum dots.

[0078] This embodiment provides a quantum dot composition, including ZnCuInSe prepared in embodiment 1 x S 2-x Quantum dots and ZnSn prepared in Example 2 y CuInS2 quantum dots, the ZnCuInSe x S 2-x Quantum dots and the ZnSn y The molar ratio of CuInS2 quantum dots is 1:0.6; wherein x=0.8, y=0.08; the quantum dot composition is obtained by mixing two quantum dots.

[0079] Comparative Example 1 The difference between this comparative example and Example 2 is that no Zn is added, and the specific steps are as follows: Preparation of S source precursor solution: 0.32 g of S powder and 10 mL of OAM were placed in a three-necked flask, heated from room temperature to 60°C and vacuum degassed, then heated from 60°C to 90°C and introduced nitrogen, and heated at 90°C for 5 min with nitrogen introduced. After being fully dissolved, the solution was vacuum degassed, cooled to room temperature, transferred to a penicillin bottle, and sealed for storage to obtain a 1 mol / L S source precursor solution.

[0080] Preparation of Sn source precursor solution: 0.2369 g of Sn powder, 2 mL of DPP and 10 mL of OAM were added to a penicillin bottle and heated in a water bath to obtain a 0.25 mol / L Sn source precursor solution. 0.1753 g of SnCl4·5H2O and 10 mL of OAM were added to a three-necked flask, heated from room temperature to 60°C for vacuum degassing, then heated from 60°C to 130°C and nitrogen was introduced to ensure that the experimental environment was oxygen-free to prevent oxidation. Nitrogen was continuously introduced and heated at 130°C for 5 min. After being fully dissolved, vacuum degassing was performed, cooled to room temperature, transferred to a penicillin bottle and sealed for storage, and a 0.05 mol / L Sn source precursor solution was obtained; Preparation of Sn / S ion mixture: sampling the prepared S source precursor solution and Sn source precursor solution according to the Sn / S molar ratio of 0.08:2, putting them into a penicillin bottle and stirring for 10 minutes for later use; Synthetic Sn 0.08CuInS2 quantum dots: 0.2 mmol of In(OAc)3, 0.14 mmol of CuI, 4 mL of OAM and 8 mL of ODE were added to a three-necked flask, vacuumed and heated to 60°C, then replaced with a N2 atmosphere and heated to 100°C. The flask was kept at 100°C for 3 min to allow the cationic reagent to fully dissolve. Vacuumed again for 2 min to ensure that there were no impurities such as oxygen and water vapor in the reaction atmosphere. The reaction system was heated under N2 atmosphere. When the temperature rose to 170°C, a total of 1 mmol of Se / S ion mixture was injected. After 15 minutes of reaction, heating was stopped, and 10 ml of petroleum ether was added after the temperature dropped to 90°C. The temperature was lowered, and the Sn was purified by centrifugation and dried to prepare the Sn2. 0.08 CuInS2 quantum dots.

[0081] The Sn prepared by doping only Sn in this comparative example 0.08 CuInS2 is easily deposited and agglomerated in dichloromethane solvent, so no further tests were performed on it.

[0082] Comparative Example 2 This comparative example proposes a quantum dot composition, including ZnCuInSe prepared in Example 1 x S 2-x Quantum dots and ZnSn prepared in Example 2 y CuInS2 quantum dots, the ZnCuInSe x S 2-x Quantum dots and the ZnSn y The molar ratio of CuInS2 quantum dots is 1:2; wherein x=0.8, y=0.08; and the quantum dot composition is obtained by mixing two quantum dots.

[0083] Table 3 Photoelectric performance parameters of the quantum dot compositions prepared in Examples 5-7 and Comparative Example 2 Sample name Voc(mV) Jsc(mA / cm2) FF η(%) Example 5 531.27 18.32 0.68 6.68 Example 6 536.16 18.85 0.67 6.83 Example 7 539.72 18.96 0.69 7.12 Comparative Example 2 469.57 14.87 0.58 4.09 It can be seen from Table 3 that the composition composed of two quantum dots in a specific ratio proposed by the present invention can significantly improve the battery efficiency, which can be as high as 7% or more, while the battery efficiency of the two quantum dots in other ratios is improved, but not significantly.

[0084] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A ZnCuInSe x S 2-x or ZnSn y The method for preparing CuInS2 quantum dots is characterized in that: The following steps are involved: The Zn source precursor solution, In(OAc)3, CuI, oleylamine and octadecene are mixed, vacuumed and heated to 55-65°C, then heated to 95-100°C in a nitrogen atmosphere and kept warm, then vacuumed again and the reaction system is heated in a nitrogen atmosphere, then heated to 160-170°C and Se / S ion mixture or Sn / S ion mixture is injected to react, then cooled to 80-90°C and petroleum ether is added to obtain ZnCuInSe x S 2-x Quantum dots or ZnSn y CuInS2 quantum dots.

2. ZnCuInSe according to claim 1 x S 2-x or ZnSn y The method for preparing CuInS2 quantum dots is characterized in that: The Zn source precursor solution is prepared by the following steps: The Zn(OAc)2, octadecene and oleylamine are mixed and heated to 55-60°C and evacuated, and then heated to 120-130°C and nitrogen is continuously introduced for heating to obtain the Zn source precursor solution.

3. ZnCuInSe according to claim 2 x S 2-x or ZnSn y The method for preparing CuInS2 quantum dots is characterized in that: The heating time at 120-130°C with nitrogen is 5-8 minutes.

4. ZnCuInSe according to claim 1 x S 2-x or ZnSn y The method for preparing CuInS2 quantum dots is characterized in that: The Se / S ion mixture or the Sn / S ion mixture is prepared by the following steps: Mix the S powder and oleylamine, heat to 55-60°C, evacuate, and then heat to 80-90°C, continuously introduce nitrogen and keep heating to obtain a S source precursor solution; Se powder, diphenylphosphine and oleylamine are mixed and heated in a water bath to obtain a Se source precursor solution; alternatively, SnCl4·5H2O and oleylamine are mixed, heated to 55-60°C for vacuum degassing, and then continued to heat to 120-130°C and continue to introduce nitrogen for heating for 5-10 minutes, and after being fully dissolved, vacuum degassing is performed to obtain a Sn source precursor solution; The S source precursor solution is mixed with the Se source precursor solution or the Sn source precursor solution to obtain the Se / S ion mixture or the Sn / S ion mixture.

5. ZnCuInSe according to claim 3 x S 2-x or ZnSn y The preparation method of CuInS2 quantum dots, the concentration of S in the S source precursor solution is 1-1.2 mol / L; the concentration of Se or Sn in the Se source precursor solution or the Sn source precursor solution is 0.25-0.35 mol / L.

6. ZnCuInSe according to claim 1 x S 2-x or ZnSn y The method for preparing CuInS2 quantum dots is characterized in that: The concentration of Zn in the Zn source precursor solution is 0.1-0.2 mol / L.

7. ZnCuInSe according to claim 1 x S 2-x or ZnSn y The method for preparing CuInS2 quantum dots is characterized in that: Heating to 95-100° C. and keeping warm for 3-10 minutes; and / or, heating to 160-170° C. and injecting Se / S ion mixture or Sn / S ion mixture for reaction for 15-20 minutes.

8. A ZnCuInSe x S 2-x or ZnSn y CuInS2 quantum dots, characterized in that The invention is prepared by the preparation method according to any one of claims 1 to 7.

9. ZnCuInSe according to claim 8 x S 2-x or ZnSn y CuInS2 quantum dots, characterized in that The value of x is 0.4-1.6, and the value of y is 0.02-0.

08.

10. A quantum dot composition, characterized in that: Comprising the ZnCuInSe according to any one of claims 8 to 9 x S 2-x Quantum dots and ZnSn y CuInS2 quantum dots, the ZnCuInSe x S 2-x Quantum dots and the ZnSn y The molar ratio of CuInS2 quantum dots is 1:(0.4-0.6); where x=0.8, y=0.08.