Method for preparing CHDM through fixed bed type PTA hydrogenation
Through the fixed-bed PTA hydrogenation method and the optimization of catalyst ratio, the efficient preparation of 1,4-cyclohexanedimethanol was achieved, and the problems of low CHDM preparation efficiency and yield in the prior art were solved, achieving high conversion and collection rate effect.
Patent Information
- Application Number
- CN202411178067.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to achieve high activity and selective preparation of 1,4-cyclohexanedimethanol (CHDM), resulting in lower industrial production efficiency and output than demand.
The fixed-bed PTA hydrogenation method is adopted, through two stages of reaction steps and optimized catalyst ratio, the temperature and pressure in the kettle are controlled, and the reaction is carried out using metal oxides and support catalysts. The reaction rate is more than 98%, and the product yield is 93% and above.
The efficient preparation of 1,4-cyclohexanedimethanol was achieved, and the raw material conversion rate and product yield reached the industry's high level, solving the problems of low efficiency and output in the existing technology.
Smart Images

Figure BDA0005011294170000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemistry, and in particular to a method for preparing CHDM by hydrogenation of PTA in a fixed bed. Background Art
[0002] 1,4-cyclohexanedimethanol (CHDM) is an important monomer for the production of modified polyester. Due to the symmetry of the molecular structure, its polyester products have better thermal stability, transparency, impact resistance, wear resistance and corrosion resistance than PET and PBT. In 2017, the global consumption of CHDM exceeded 200,000 tons / year, and it grew at an average annual rate of 10%. The main producers include Eastman in the United States, Mitsubishi in Japan, SK in South Korea and other companies, and their products are almost not sold to the outside world. my country's current demand for CHDM is 50,000 tons / year, and only Kailing Chemical has a production capacity of 20,000 tons / year and Jiangsu Kangheng Chemical has a production capacity of 2,000 tons / year. The actual output is less than 10,000 tons / year, and there is a large gap. At present, the industrial production of CHDM mainly uses dimethyl terephthalate as raw material, and is carried out in two steps of benzene ring hydrogenation and ester group hydrogenation.
[0003] Regarding the hydrogenation of benzene ring and ester group in the preparation of 1,4-cyclohexanedimethanol from DMT, how to achieve high activity and high selectivity in the preparation of CHDM has become a research hotspot. Summary of the invention
[0004] The object of the present invention is to provide a fixed-bed method for preparing CHDM by hydrogenation of PTA to solve the above-mentioned problems in the prior art.
[0005] The present invention discloses a method for preparing CHDM by hydrogenation of PTA in a fixed bed, comprising the following steps:
[0006] S1, first stage reaction: pre-add the prepared mixture of PTA and solvent into the raw material tank, the concentration of PTA in the mixture is 5%-10%, then nitrogen replacement and air tightness test of the device are carried out after the prepared catalyst is loaded, and the fixed bed and preheater are heated to the reaction temperature of 200-240°C, and the pressure reducing valve is adjusted to the reaction pressure of 6-12MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.2-0.5 at the air velocity and 60-150 at the hydrogen-oil molar ratio. After the reaction is completed, the first stage reactant 1,4-cyclohexanedicarboxylic acid is obtained;
[0007] S2, two-stage reaction: pre-add the mixture consisting of the first-stage reactant and the solvent into the raw material tank, the concentration of the first-stage reactant in the mixture is 5%-10%, and then the prepared catalyst is loaded and nitrogen replacement and the air tightness test of the device are carried out. After completion, the fixed bed and the preheater are heated to the reaction temperature of 240-260°C, and the pressure reducing valve is adjusted to the reaction pressure of 10-12MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.15-0.5 space velocity and 90-160 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained.
[0008] Furthermore, the solvents in the first-stage reaction and the second-stage reaction are water, methanol or isopropanol.
[0009] Furthermore, the catalyst used in the first stage reaction includes a metal oxide and a carrier;
[0010] The metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are: Ru 0.5-1wt%, Pd 3-5-wt%, Sn 1-2wt%;
[0011] The carrier is one of activated carbon, molecular sieve and alumina.
[0012] Furthermore, the catalyst used in the second-stage reaction includes a metal oxide and a carrier;
[0013] The metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are: Ru2-5wt%, Mg0.5-1wt%, Sn5-10wt%, Pt1-2wt% respectively;
[0014] The carrier is one of activated carbon, molecular sieve and alumina.
[0015] The invention also discloses CHDM, which is prepared by the method.
[0016] Beneficial effects of the present invention: By adopting the method of the present invention, by selecting a suitable catalyst and optimizing the ratio of each component in the catalyst, the temperature and pressure in the kettle are reasonably controlled, so that the raw material conversion rate reaches and exceeds 98%, and the product yield is also 93% and above, which is at a relatively high level in the industry. DETAILED DESCRIPTION
[0017] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0018] Example 1
[0019] S1, first stage reaction: pre-add the prepared mixture of PTA and solvent into the raw material tank, the concentration of PTA in the mixture is 5%, then nitrogen replacement and air tightness test of the device are carried out after the prepared catalyst is loaded, and after completion, the fixed bed and preheater are heated to the reaction temperature of 200°C, and the pressure reducing valve is adjusted to the reaction pressure of 6MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.2 space velocity and 60 hydrogen-to-oil molar ratio. After the reaction is completed, the first stage reactant 1,4-cyclohexanedicarboxylic acid is obtained; the raw material conversion rate is 98%, and the product yield is 95%;
[0020] S2, two-stage reaction: add a mixture consisting of a first-stage reactant and a solvent into the raw material tank in advance, the concentration of the first-stage reactant in the mixture is 5%, and then carry out nitrogen replacement and device air tightness test after the prepared catalyst is loaded. After completion, the fixed bed and the preheater are heated to a reaction temperature of 240°C, and the pressure reducing valve is adjusted to a reaction pressure of 10MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.15 space velocity and 90 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained; the raw material conversion rate is 99%, and the product yield is 98%.
[0021] Wherein, the solvents in the first-stage reaction and the second-stage reaction are both water or methanol or isopropanol; the catalyst used in the first-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are respectively: Ru0.5-1wt%, Pd3-5-wt%, Sn1-2wt%, and the carrier is activated carbon; the catalyst used in the second-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are respectively: Ru2-5wt%, Mg05-1wt%, Sn5-10wt%, Pt1-2wt%, and the carrier is activated carbon.
[0022] Example 2
[0023] S1, first stage reaction: pre-add the prepared mixture of PTA and solvent into the raw material tank, the concentration of PTA in the mixture is 5%, then nitrogen replacement and air tightness test of the device are carried out after the prepared catalyst is loaded, after completion, the fixed bed and preheater are heated to the reaction temperature of 220°C, the pressure reducing valve is adjusted to the reaction pressure of 6MPa, after the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, the hydrogen flow rate is adjusted, the space velocity is 0.2, and the hydrogen-to-oil molar ratio is 60, after the reaction is completed, the first stage reactant 1,4-cyclohexanedicarboxylic acid is obtained; the raw material conversion rate is 99.5%, and the product yield is 94%;
[0024] S2, two-stage reaction: add a mixture consisting of a first-stage reactant and a solvent into the raw material tank in advance, the concentration of the first-stage reactant in the mixture is 5%, and then carry out nitrogen replacement and device air tightness test after the prepared catalyst is loaded. After completion, the fixed bed and the preheater are heated to a reaction temperature of 260°C, and the pressure reducing valve is adjusted to a reaction pressure of 10MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.15 space velocity and 90 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained; the raw material conversion rate is 99.8%, and the product yield is 97%.
[0025] Wherein, the solvents in the first-stage reaction and the second-stage reaction are both water or methanol or isopropanol; the catalyst used in the first-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are: Ru0.5-1wt%, Pd3-5-wt%, Sn1-2wt%, and the carrier is γ-alumina; the catalyst used in the second-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are: Ru2-5wt%, Mg05-1wt%, Sn5-10wt%, Pt1-2wt%, and the carrier is γ-alumina.
[0026] Example 3
[0027] S1, first stage reaction: pre-add the prepared mixture of PTA and solvent into the raw material tank, the concentration of PTA in the mixture is 5%, then nitrogen replacement and device air tightness test are carried out after the prepared catalyst is loaded, and after completion, the fixed bed and preheater are heated to the reaction temperature of 200°C, and the pressure reducing valve is adjusted to the reaction pressure of 12MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.2 space velocity and 60 hydrogen-to-oil molar ratio. After the reaction is completed, the first stage reactant 1,4-cyclohexanedicarboxylic acid is obtained; the raw material conversion rate is 99%, and the product yield is 98%;
[0028] S2, two-stage reaction: pre-add a mixture consisting of a first-stage reactant and a solvent into the raw material tank, the concentration of the first-stage reactant in the mixture is 5%, and then the prepared catalyst is loaded and nitrogen replacement and the air tightness test of the device are carried out. After completion, the fixed bed and the preheater are heated to a reaction temperature of 240°C, and the pressure reducing valve is adjusted to a reaction pressure of 12MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.15 space velocity and 90 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained; the raw material conversion rate is 99%, and the product yield is 98.5%.
[0029] Wherein, the solvents in the first-stage reaction and the second-stage reaction are both water or methanol or isopropanol; the catalyst used in the first-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are: Ru0.5-1wt%, Pd3-5-wt%, Sn1-2wt%, and the carrier is a molecular sieve; the catalyst used in the second-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are: Ru2-5wt%, Mg05-1wt%, Sn5-10wt%, Pt1-2wt%, and the carrier is a molecular sieve.
[0030] Example 4
[0031] S1, first stage reaction: pre-add the prepared mixture of PTA and solvent into the raw material tank, the concentration of PTA in the mixture is 5%, then nitrogen replacement and air tightness test of the device are carried out after the prepared catalyst is loaded, and the fixed bed and preheater are heated to the reaction temperature of 200°C, and the pressure reducing valve is adjusted to the reaction pressure of 6MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.5 space velocity and 60 hydrogen-to-oil molar ratio. After the reaction is completed, the first stage reactant 1,4-cyclohexanedicarboxylic acid is obtained; the raw material conversion rate is 98%, and the product yield is 93%;
[0032] S2, two-stage reaction: add a mixture consisting of a first-stage reactant and a solvent into the raw material tank in advance, the concentration of the first-stage reactant in the mixture is 5%, and then carry out nitrogen replacement and device air tightness test after the prepared catalyst is loaded. After completion, the fixed bed and the preheater are heated to a reaction temperature of 240°C, and the pressure reducing valve is adjusted to a reaction pressure of 10MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.5 space velocity and 90 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained; the raw material conversion rate is 99.5%, and the product yield is 98.8%.
[0033] Wherein, the solvents in the first-stage reaction and the second-stage reaction are both water or methanol or isopropanol; the catalyst used in the first-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are: Ru0.5-1wt%, Pd3-5-wt%, Sn1-2wt%, and the carrier is γ-alumina; the catalyst used in the second-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are: Ru2-5wt%, Mg05-1wt%, Sn5-10wt%, Pt1-2wt%, and the carrier is γ-alumina.
[0034] Example 5
[0035] S1, first stage reaction: pre-add the prepared mixture of PTA and solvent into the raw material tank, the concentration of PTA in the mixture is 5%, then nitrogen replacement and device air tightness test are carried out after the prepared catalyst is loaded, and after completion, the fixed bed and preheater are heated to the reaction temperature of 200°C, and the pressure reducing valve is adjusted to the reaction pressure of 6MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.2 space velocity and 90 hydrogen-to-oil molar ratio. After the reaction is completed, the first stage reactant 1,4-cyclohexanedicarboxylic acid is obtained; the raw material conversion rate is 99.5%, and the product yield is 99%;
[0036] S2, two-stage reaction: add a mixture consisting of a first-stage reactant and a solvent into the raw material tank in advance, the concentration of the first-stage reactant in the mixture is 5%, and then carry out nitrogen replacement and device air tightness test after the prepared catalyst is loaded. After completion, the fixed bed and the preheater are heated to a reaction temperature of 240°C, and the pressure reducing valve is adjusted to a reaction pressure of 10MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.15 space velocity and 160 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained; the raw material conversion rate is 99.8%, and the product yield is 99%.
[0037] Wherein, the solvents in the first-stage reaction and the second-stage reaction are both water or methanol or isopropanol; the catalyst used in the first-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are respectively: Ru0.5-1wt%, Pd3-5-wt%, Sn1-2wt%, and the carrier is activated carbon; the catalyst used in the second-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are respectively: Ru2-5wt%, Mg05-1wt%, Sn5-10wt%, Pt1-2wt%, and the carrier is activated carbon.
[0038] Example 6
[0039] S1, first stage reaction: pre-add the prepared mixture of PTA and solvent into the raw material tank, the concentration of PTA in the mixture is 10%, then nitrogen replacement and air tightness test of the device are carried out after the prepared catalyst is loaded, and the fixed bed and preheater are heated to the reaction temperature of 200°C, and the pressure reducing valve is adjusted to the reaction pressure of 6MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.2 space velocity and 60 hydrogen-to-oil molar ratio. After the reaction is completed, the first stage reactant 1,4-cyclohexanedicarboxylic acid is obtained; the raw material conversion rate is 98%, and the product yield is 93%;
[0040] S2, two-stage reaction: add a mixture consisting of a first-stage reactant and a solvent into the raw material tank in advance, the concentration of the first-stage reactant in the mixture is 10%, and then carry out nitrogen replacement and device air tightness test after the prepared catalyst is loaded. After completion, the fixed bed and the preheater are heated to a reaction temperature of 240°C, and the pressure reducing valve is adjusted to a reaction pressure of 10MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.15 space velocity and 90 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained; the raw material conversion rate is 98%, and the product yield is 96%.
[0041] The solvents in the first-stage reaction and the second-stage reaction are water, methanol or isopropanol; the catalyst used in the first-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are: Ru0.5-1wt%, Pd3-5-wt%, Sn1-2wt%, and the carrier is γ-alumina; the catalyst used in the second-stage reaction includes a metal oxide and a carrier; the metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are: Ru2-5wt%, Mg0.5-1wt%, Sn5-10wt%, Pt1-2wt%, and the carrier is γ-alumina. 。
[0042] The data of the above test process are as follows:
[0043]
[0044] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing CHDM by hydrogenation of PTA in a fixed bed, characterized in that: The following steps are involved: S1, a first-stage reaction: pre-add the prepared mixture of PTA and solvent into the fixed bed, the concentration of PTA in the mixture is 5%-10%, and then the prepared catalyst is loaded and nitrogen replacement and device air tightness test are performed. After completion, the fixed bed and preheater are heated to a reaction temperature of 200-240°C, and the pressure reducing valve is adjusted to a reaction pressure of 8-12MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.2-0.5 at an air velocity and a hydrogen-to-oil molar ratio of 60-150. After the reaction is completed, a first-stage reactant 1,4-cyclohexanedicarboxylic acid is obtained; S2, two-stage reaction: add a mixture consisting of a first-stage reactant and a solvent into the fixed bed in advance, the concentration of the first-stage reactant in the mixture is 5%-10%, and then carry out nitrogen replacement and device air tightness test after the prepared catalyst is loaded. After completion, the fixed bed and the preheater are heated to a reaction temperature of 240-260°C, and the pressure reducing valve is adjusted to a reaction pressure of 10-12MPa. After the temperature and pressure are stable, the feed pump is turned on to start feeding 1-10ml / min, and the hydrogen flow rate is adjusted to 0.15-0.5 space velocity and 90-160 hydrogen-to-oil molar ratio. After the reaction is completed, 1,4-cyclohexanedimethanol can be obtained.
2. The method for preparing CHDM by hydrogenation of PTA in a fixed bed according to claim 1, characterized in that: The solvents in the first-stage reaction and the second-stage reaction are water, methanol or isopropanol.
3. The method for preparing CHDM by hydrogenation of PTA in a fixed bed according to claim 1, characterized in that: The catalyst used in the first stage reaction includes a metal oxide and a carrier; The metal elements in the metal oxide include Ru, Pd and Sn, and the mass fractions of the metal elements in the metal oxide are: Ru 0.5-1wt%, Pd 3-5-wt%, Sn 1-2wt%; The carrier is one of activated carbon, molecular sieve and alumina.
4. The method for preparing CHDM by hydrogenation of PTA in a fixed bed according to claim 3, characterized in that: The catalyst used in the second-stage reaction includes a metal oxide and a carrier; The metal elements in the metal oxide include Ru, Mg, Sn and Pt, and the mass fractions of the metal elements in the metal oxide are: Ru2-5wt%, Mg05-1wt%, Sn5-10wt%, Pt1-2wt% respectively; The carrier is one of activated carbon, molecular sieve and alumina.
5. A CHDM, characterized in that: The method according to any one of claims 1 to 4 is adopted to prepare the present invention.