Adhesive for rubber, rubber compound and preparation method thereof

By controlling the oil absorption value and dispersion of white carbon black, a highly dispersible rubber adhesive was prepared, which solved the problem of unstable compounding of HMMM-65 adhesives in the prior art, and improved the rheology of the mixing rubber Stability and consistency in use.

CN119081607APending Publication Date: 2024-12-06GUIZHOU TIRE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411395439.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The hexamethoxymethylmelamine-65 (HMM-65) adhesive used in the current tire industry does not control the oil absorption of white carbon black during the compounding process, resulting in large differences in the use effect of different manufacturers and stable rheology. Poor sex.

Method used

By controlling the oil absorption value of white carbon black between 1-5.4cm3/g, and using high-dispersed white carbon black, ensuring that its dispersion in rubber reaches level 9.5 or above, a new type of rubber adhesive was prepared and combined with natural rubber , carbon black reinforcement agent, chemical additive and other components to prepare kneaded glue to improve rheology stability.

Benefits of technology

It significantly improves the rheology stability performance of the mixing glue, reduces the use differences between different manufacturers, and improves the bonding effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides an adhesive for rubber, a rubber compound and a preparation method of the rubber compound. The adhesive for the rubber comprises hexamethoxymethyl melamine and white carbon black, the oil absorption value of the white carbon black is 1-5.4 cm < 3 > / g, and the dispersion degree of the white carbon black in the rubber reaches more than 9.5 level; the applicant researches the used compounded white carbon black and controls the oil absorption value and dispersity of the white carbon black, so that the novel adhesive for rubber is compounded, and the adhesive is used for rubber hanging of a tire steel wire to improve the rheological stability of a rubber compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of tires, and in particular to a rubber adhesive, a rubber compound and a preparation method thereof. Background Art

[0002] Since the tire industry uses a lot of steel wire rubber in the full steel tire series, hexamethoxymethylmelamine-65, also known as rubber adhesive RA-65 (i.e. HMMM-65): is a compound of 65% hexamethoxymethylmelamine (HMMM) and a carrier, which is a methylene donor adhesive. It is used in conjunction with a methylene acceptor to bond rubber to skeleton materials such as steel wire. However, the HMMM-65 currently used by tire companies generally uses 35% of ordinary nitrogen adsorption specific surface area of ​​175 white carbon black and 100% of liquid HMMM to compound into a solid for easy feeding. Generally, the oil absorption of white carbon black is not controlled during compounding, resulting in the use of HMMM-65 from different manufacturers in the steel wire rubber compound. Due to poor dispersion of the same manufacturer, the fluctuation is large, and the compounding of different manufacturers is large. The fluctuation between manufacturers is also large. In addition, the failure to control the oil absorption of white carbon black leads to poor rheological stability of the rubber adhesive.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] In view of this, the present invention proposes a rubber adhesive, a rubber compound and a preparation method thereof to solve the technical defects existing in the prior art.

[0005] In a first aspect, the present invention provides a rubber adhesive comprising the following components in parts by weight:

[0006] 20-80 parts of hexamethoxymethylmelamine, 20-80 parts of white carbon black;

[0007] The oil absorption value of the white carbon black is 1 to 5.4 cm 3 / g, the white carbon black is a highly dispersed white carbon black, and the white carbon black is a white carbon black with a dispersion degree of 9.5 or above in the rubber.

[0008] Preferably, the oil absorption value of the white carbon black is 4.4 cm 3 / g.

[0009] In a second aspect, the present invention further provides a rubber compound, comprising: natural rubber, a carbon black reinforcing agent, white carbon black, a chemical additive, and an adhesive;

[0010] Wherein, the adhesive is the adhesive described above.

[0011] Preferably, it comprises the following components by weight: 70-100 parts of natural rubber, 20-80 parts of carbon black reinforcing agent, 15-25 parts of white carbon black, 5-20 parts of chemical additives, and 1-10 parts of adhesive;

[0012] The oil absorption value of the white carbon black in the rubber compound is 1 to 5.4 cm 3 / g, the white carbon black is highly dispersed white carbon black or ordinary white carbon black;

[0013] The highly dispersed white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber;

[0014] The ordinary white carbon black is white carbon black with a dispersion degree in rubber lower than grade 9.5.

[0015] Preferably, the chemical additives include at least two of an antioxidant, a vulcanizing agent, an accelerator and zinc oxide.

[0016] Preferably, the antioxidant includes antioxidant RD and / or antioxidant 4020;

[0017] And / or, the accelerator includes accelerator D and / or accelerator CZ;

[0018] And / or, the vulcanizing agent is sulfur.

[0019] Preferably, the chemical additives include the following components in parts by weight: 1 to 3 parts of antioxidant, 1 to 3 parts of vulcanizing agent, 1.5 to 2 parts of accelerator, and 5 to 10 parts of zinc oxide.

[0020] In a third aspect, the present invention further provides a method for preparing the rubber compound, comprising the following steps:

[0021] The natural rubber is placed in an internal mixer and mixed to obtain plastic;

[0022] The plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive are mixed in an internal mixer; then the material is discharged to an open mixer after the plug is pressed, and the material is turned over and cooled. After adding the vulcanizing agent and accelerator, the material is thinly passed, and the material is cooled to obtain a mixed rubber.

[0023] Preferably, the natural rubber is placed in an internal mixer, the speed of the internal mixer is set to 30-55 rpm, the plug is pressed for 55-60 seconds, the plug is lifted and kept for 20-25 seconds, and then the plug is pressed to 160-165° C. and then the material is discharged to obtain the plastic;

[0024] The plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive are placed in an internal mixer, and the speed of the internal mixer is set to 30-55 rpm. After pressing the bolt for 25-30 seconds, the bolt is lifted and held for 3-5 seconds, and then the bolt is pressed to 130-135°C and the bolt is lifted and held for 15-20 seconds; then the bolt is pressed to 150-155°C and then discharged to an open mixer, and the mixture is cooled to 90-100°C, and the vulcanizer and accelerator are added and thinned for 200-300 seconds, and the mixture is cooled to obtain a mixed rubber.

[0025] The rubber adhesive of the present invention has the following beneficial effects compared with the prior art:

[0026] The rubber adhesive of the present invention comprises hexamethoxymethyl melamine and white carbon black, wherein the oil absorption value of the white carbon black is 1 to 5.4 cm 3 / g, the applicant studied the use of compounded white carbon black, controlled the oil absorption value and dispersibility of white carbon black, and compounded a new type of rubber adhesive for use in tire steel wire rubber coating to improve the rheological stability of the mixed rubber. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present application provides a rubber adhesive, comprising the following components in parts by weight: 20 to 80 parts of hexamethoxymethylmelamine and 20 to 80 parts of white carbon black;

[0029] Among them, the oil absorption value of white carbon black is 1 to 5.4 cm 3 / g; white carbon black is highly dispersed white carbon black. Highly dispersed white carbon black is defined as follows: According to GB / T32678-2016, it is obtained by neutralizing a silicate solution with an acid under certain conditions and undergoing a precipitation reaction. It is a white inorganic material in the form of amorphous particles; white carbon black with a dispersion degree of 9.5 or above in rubber.

[0030] The rubber adhesive of the present invention comprises hexamethoxymethyl melamine and white carbon black, wherein the oil absorption value of the white carbon black is 1 to 5.4 cm 3 / g, the applicant studied the use of compounded white carbon black, controlled the oil absorption value and dispersibility of white carbon black, and compounded a new type of rubber adhesive for use in tire steel wire coating to improve the rheological stability of the mixed rubber.

[0031] In some embodiments, the oil absorption value of white carbon is 4.4 cm 3 / g.

[0032] Based on the same inventive concept, the present invention also provides a rubber compound, comprising: natural rubber, carbon black reinforcing agent, white carbon black, chemical additives, and adhesive;

[0033] Wherein, the adhesive is the above-mentioned adhesive.

[0034] The rubber mix of the present invention includes the above-mentioned rubber adhesive. The above-mentioned rubber adhesive is used to replace the original compound for tire steel wire coating and can be used in the rubber mix to improve the rheological stability of the rubber mix.

[0035] In some embodiments, the rubber mix includes the following components by weight: 70-100 parts of natural rubber, 20-80 parts of carbon black reinforcing agent, 15-25 parts of white carbon black, 5-20 parts of chemical additives, and 1-10 parts of adhesive;

[0036] The oil absorption value of white carbon black in the rubber compound is 1 to 5.4 cm 3 / g, white carbon black is highly dispersed white carbon black or ordinary white carbon black;

[0037] Highly dispersed white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber;

[0038] Ordinary white carbon black is white carbon black with a dispersion degree in rubber lower than grade 9.5.

[0039] Specifically, ordinary white carbon black is defined as follows: According to GB / T32678-2016, it is obtained by neutralizing a silicate solution with an acid under certain conditions and causing a precipitation reaction, and it exists in the form of amorphous particles in white inorganic materials; white carbon black with a dispersion degree in rubber lower than level 9.5.

[0040] In some embodiments, the chemical additive includes the following components in parts by weight: 1 to 3 parts of antioxidant, 1 to 3 parts of vulcanizing agent, 1.5 to 2 parts of accelerator, and 5 to 10 parts of zinc oxide.

[0041] In some embodiments, the antioxidant includes antioxidant RD and / or antioxidant 4020; specifically, antioxidant RD, also known as antioxidant RD, antioxidant 224, the molecular formula is C 12 H 17 N; Antioxidant 4020, also known as antioxidant DMPPD, has a molecular formula of C 18 H 24 N2.

[0042] In some embodiments, the accelerator includes accelerator D and / or accelerator CZ; accelerator D, also known as diphenylguanidine, has a molecular formula of C 13 H 13 N3; accelerator CZ, chemical name N-cyclohexyl-2-benzothiazole sulfenamide, molecular formula C13 H 16 N2S2.

[0043] In some embodiments, the vulcanizing agent is sulfur.

[0044] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned rubber compound, comprising the following steps:

[0045] S1, mixing natural rubber in an internal mixer to obtain plastic;

[0046] S2. Mix plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive in an internal mixer; then discharge the material to an open mixer after pressing the plug, mix and cool, add vulcanizing agent and accelerator, and then thinly pass, cool down and obtain a mixed rubber.

[0047] In some embodiments, natural rubber is placed in an internal mixer, the speed of the internal mixer is set to 30-55 rpm, the plug is pressed for 55-60 seconds, the plug is lifted and kept for 20-25 seconds, and then the plug is pressed to 160-165° C. and then the material is discharged to obtain plastic;

[0048] The plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive are placed in an internal mixer, and the speed of the internal mixer is set to 30-55 rpm. After pressing the bolt for 25-30 seconds, the bolt is lifted and held for 3-5 seconds, and then the bolt is pressed to 130-135°C and the bolt is lifted and held for 15-20 seconds; then the bolt is pressed to 150-155°C and then discharged to an open mixer, and the mixture is cooled to 90-100°C, and the vulcanizer and accelerator are added and thinned for 200-300 seconds, and the mixture is cooled to obtain a mixed rubber.

[0049] The following further describes the rubber adhesive, rubber compound and preparation method of the present application with specific examples. This section further describes the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means adopted in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0050] In the following examples, the carbon black reinforcing agent is a black cat carbon black reinforcing agent (purchased from Jiangxi Black Cat Carbon Black Co., Ltd.), model N234.

[0051] Example 1

[0052] This embodiment provides a rubber adhesive, comprising the following components in parts by weight: 40 parts of hexamethoxymethylmelamine and 40 parts of white carbon black;

[0053] Among them, white carbon black is highly dispersed white carbon black, white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber, and the oil absorption value of white carbon black is 4.4cm3 / g;

[0054] This embodiment also provides a rubber compound, comprising the following components by weight: 80 parts of natural rubber, 60 parts of carbon black reinforcing agent, white carbon black (white carbon black is ordinary white carbon black, with an oil absorption value of 2.8 cm 3 / g) 20 parts, adhesive 4 parts, antioxidant 2 parts, vulcanizing agent 2 parts, accelerator 1.7 parts, zinc oxide 8 parts;

[0055] Wherein, the adhesive is the adhesive in Example 1;

[0056] The antioxidant is antioxidant RD;

[0057] The accelerator is accelerator CZ;

[0058] The vulcanizing agent is sulfur.

[0059] The preparation method of the above-mentioned rubber compound comprises the following steps:

[0060] S1. Place the natural rubber in an internal mixer, set the mixer speed to 30 rpm, press the plug for 60 seconds, lift the plug and keep it for 20 seconds, then press the plug to 165°C and discharge the material to obtain plastic;

[0061] S2. Place plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive in an internal mixer, set the speed of the internal mixer to 30 rpm, press the bolt for 30 seconds, lift the bolt and hold it for 5 seconds, then press the bolt to 135°C and lift the bolt and hold it for 20 seconds; then press the bolt to 155°C and discharge it to an open mixer, refining and cooling to 100°C, adding vulcanizer and accelerator, thinning for 300 seconds, cooling the sheet down to obtain a mixed rubber.

[0062] Example 2

[0063] This embodiment provides a rubber adhesive, comprising the following components in parts by weight: 40 parts of hexamethoxymethylmelamine and 40 parts of white carbon black;

[0064] Among them, white carbon black is highly dispersed white carbon black, white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber, and the oil absorption value of white carbon black is 2.3cm 3 / g.

[0065] This embodiment also provides a rubber compound, comprising the following components by weight: 80 parts of natural rubber, 60 parts of carbon black reinforcing agent, white carbon black (white carbon black is ordinary white carbon black, with an oil absorption value of 2.8 cm 3 / g) 20 parts, adhesive 4 parts, antioxidant 2 parts, vulcanizing agent 2 parts, accelerator 1.7 parts, zinc oxide 8 parts;

[0066] Wherein, the adhesive is the adhesive in Example 2;

[0067] The antioxidant is antioxidant RD;

[0068] The accelerator is accelerator CZ;

[0069] The vulcanizing agent is sulfur.

[0070] The preparation method of the above-mentioned rubber compound comprises the following steps:

[0071] S1. Place the natural rubber in an internal mixer, set the mixer speed to 30 rpm, press the plug for 60 seconds, lift the plug and keep it for 20 seconds, then press the plug to 165°C and discharge the material to obtain plastic;

[0072] S2. Place plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive in an internal mixer, set the speed of the internal mixer to 30 rpm, press the bolt for 30 seconds, lift the bolt and hold it for 5 seconds, then press the bolt to 135°C and lift the bolt and hold it for 20 seconds; then press the bolt to 155°C and discharge it to an open mixer, refining and cooling to 100°C, adding vulcanizer and accelerator, thinning for 300 seconds, cooling the sheet down to obtain a mixed rubber.

[0073] Example 3

[0074] This embodiment provides a rubber adhesive, comprising the following components in parts by weight: 40 parts of hexamethoxymethylmelamine and 40 parts of white carbon black;

[0075] Among them, white carbon black is ordinary white carbon black, and the oil absorption value of white carbon black is 2.3cm 3 / g; Ordinary white carbon black is defined as follows: According to GB / T32678-2016, it is obtained by neutralizing a silicate solution with an acid under certain conditions and causing a precipitation reaction, and it exists in the form of amorphous particles in white inorganic materials; white carbon black with a dispersion degree in rubber lower than grade 9.5.

[0076] This embodiment also provides a rubber compound, comprising the following components by weight: 80 parts of natural rubber, 60 parts of carbon black reinforcing agent, white carbon black (white carbon black is ordinary white carbon black, with an oil absorption value of 2.8 cm 3 / g) 20 parts, adhesive 4 parts, antioxidant 2 parts, vulcanizing agent 2 parts, accelerator 1.7 parts, zinc oxide 8 parts;

[0077] Wherein, the adhesive is the adhesive in Example 3;

[0078] The antioxidant is antioxidant RD;

[0079] The accelerator is accelerator CZ;

[0080] The vulcanizing agent is sulfur.

[0081] The preparation method of the above-mentioned rubber compound comprises the following steps:

[0082] S1. Place the natural rubber in an internal mixer, set the mixer speed to 30 rpm, press the plug for 60 seconds, lift the plug and keep it for 20 seconds, then press the plug to 165°C and discharge the material to obtain plastic;

[0083] S2. Place plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive in an internal mixer, set the speed of the internal mixer to 30 rpm, press the bolt for 30 seconds, lift the bolt and hold it for 5 seconds, then press the bolt to 135°C and lift the bolt and hold it for 20 seconds; then press the bolt to 155°C and discharge it to an open mixer, refining and cooling to 100°C, adding vulcanizer and accelerator, thinning for 300 seconds, cooling the sheet down to obtain a mixed rubber.

[0084] Example 4

[0085] This embodiment provides a rubber adhesive, comprising the following components in parts by weight: 40 parts of hexamethoxymethylmelamine and 40 parts of white carbon black;

[0086] Among them, white carbon black is highly dispersed white carbon black, white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber, and the oil absorption value of white carbon black is 3.3cm 3 / g.

[0087] This embodiment also provides a rubber compound, including the following components by weight: 80 parts of natural rubber, 60 parts of carbon black reinforcing agent, white carbon black (white carbon black is ordinary white carbon black, the oil absorption value is 2.8cm 3 / g) 20 parts, adhesive 4 parts, antioxidant 2 parts, vulcanizing agent 2 parts, accelerator 1.7 parts, zinc oxide 8 parts;

[0088] Wherein, the adhesive is the adhesive in Example 4;

[0089] The antioxidant is antioxidant RD;

[0090] The accelerator is accelerator CZ;

[0091] The vulcanizing agent is sulfur.

[0092] The preparation method of the above-mentioned rubber compound comprises the following steps:

[0093] S1. Place the natural rubber in an internal mixer, set the mixer speed to 30 rpm, press the bolt for 60 seconds, lift the bolt and keep it for 20 seconds, then press the bolt to 165°C and discharge the material to obtain plastic;

[0094] S2. Place plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive in an internal mixer, set the speed of the internal mixer to 30 rpm, press the bolt for 30 seconds, lift the bolt and hold it for 5 seconds, then press the bolt to 135°C and lift the bolt and hold it for 20 seconds; then press the bolt to 155°C and discharge it to an open mixer, refining and cooling to 100°C, adding vulcanizer and accelerator, thinning for 300 seconds, cooling the sheet down to obtain a mixed rubber.

[0095] Example 5

[0096] This embodiment provides a rubber adhesive, comprising the following components in parts by weight: 40 parts of hexamethoxymethylmelamine and 40 parts of white carbon black;

[0097] Among them, white carbon black is highly dispersed white carbon black, white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber, and the oil absorption value of white carbon black is 5cm 3 / g.

[0098] This embodiment also provides a rubber compound, including the following components by weight: 80 parts of natural rubber, 60 parts of carbon black reinforcing agent, white carbon black (white carbon black is ordinary white carbon black, the oil absorption value is 2.8cm 3 / g) 20 parts, adhesive 4 parts, antioxidant 2 parts, vulcanizing agent 2 parts, accelerator 1.7 parts, zinc oxide 8 parts;

[0099] Wherein, the adhesive is the adhesive in Example 5;

[0100] The antioxidant is antioxidant RD;

[0101] The accelerator is accelerator CZ;

[0102] The vulcanizing agent is sulfur.

[0103] The preparation method of the above-mentioned rubber compound comprises the following steps:

[0104] S1. Place the natural rubber in an internal mixer, set the mixer speed to 30 rpm, press the bolt for 60 seconds, lift the bolt and keep it for 20 seconds, then press the bolt to 165°C and discharge the material to obtain plastic;

[0105] S2. Place plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive in an internal mixer, set the speed of the internal mixer to 30 rpm, press the bolt for 30 seconds, lift the bolt and hold it for 5 seconds, then press the bolt to 135°C and lift the bolt and hold it for 20 seconds; then press the bolt to 155°C and discharge it to an open mixer, refining and cooling to 100°C, adding vulcanizer and accelerator, thinning for 300 seconds, cooling the sheet down to obtain a mixed rubber.

[0106] Example 6

[0107] This embodiment provides a rubber adhesive, comprising the following components in parts by weight: 40 parts of hexamethoxymethylmelamine and 40 parts of white carbon black;

[0108] Among them, white carbon black is highly dispersed white carbon black, white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber, and the oil absorption value of white carbon black is 5.4cm 3 / g.

[0109] This embodiment also provides a rubber compound, comprising the following components by weight: 80 parts of natural rubber, 60 parts of carbon black reinforcing agent, white carbon black (white carbon black is ordinary white carbon black, with an oil absorption value of 2.8 cm 3 / g) 20 parts, adhesive 4 parts, antioxidant 2 parts, vulcanizing agent 2 parts, accelerator 1.7 parts, zinc oxide 8 parts;

[0110] Wherein, the adhesive is the adhesive in Example 6;

[0111] The antioxidant is antioxidant RD;

[0112] The accelerator is accelerator CZ;

[0113] The vulcanizing agent is sulfur.

[0114] The preparation method of the above-mentioned rubber compound comprises the following steps:

[0115] S1. Place the natural rubber in an internal mixer, set the mixer speed to 30 rpm, press the plug for 60 seconds, lift the plug and keep it for 20 seconds, then press the plug to 165°C and discharge the material to obtain plastic;

[0116] S2. Place plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive in an internal mixer, set the speed of the internal mixer to 30 rpm, press the bolt for 30 seconds, lift the bolt and hold it for 5 seconds, then press the bolt to 135°C and lift the bolt and hold it for 20 seconds; then press the bolt to 155°C and discharge it to an open mixer, refining and cooling to 100°C, adding vulcanizer and accelerator, thinning for 300 seconds, cooling the sheet down to obtain a mixed rubber.

[0117] Performance Testing

[0118] The mixed rubbers in Examples 1 to 6 were subjected to rheological tests, specifically, the MH (maximum torque, unit dNm) value and the T50 value (unit second) were tested; wherein the MH and T50 values ​​were measured according to GB / T 16584, and the test results are shown in Table 1 below.

[0119] Table 1 - Rheological properties of rubber compounds

[0120]

[0121]

[0122] The MH value fluctuation and T50 value fluctuation of the rubber compounds in Examples 1 to 6 are shown in Table 2 below.

[0123] Table 2 - Fluctuation of MH value and T50 value of rubber compound

[0124]

[0125] The calculation method of MH value fluctuation in Table 2 is: first calculate the average and standard deviation of MH values ​​of 9 tests with different schemes, and the MH value fluctuation is equal to 3 times the standard deviation divided by the average value; the calculation method of T50 value fluctuation is: first calculate the average and standard deviation of T50 values ​​of 9 tests with different schemes, and the T50 value fluctuation is equal to 3 times the standard deviation divided by the average value.

[0126] As can be seen from Tables 1 to 2, highly dispersed white carbon black (according to GB / T32678-2016, under certain conditions, silicate solution is neutralized with acid, and precipitation reaction is obtained, and amorphous particles exist in the white inorganic material; white carbon black with a dispersion degree of 9.5 or above in rubber) fluctuates less than that of the adhesive compounded with ordinary white carbon black; then the oil absorption values ​​of white carbon black are compared. In Example 1, when the oil absorption value of highly dispersed white carbon black is 4.4 cm 3 / g, the fluctuation value of MH and T50 is the best. If the oil absorption value is increased, the processing cost of white carbon black is high, and the fluctuation range is not large. The produced adhesive may adhere to the transportation pipeline. It is preferred to use an oil absorption value of 4.4cm 3 / g of highly dispersed silica is used as the composite carrier.

[0127] The above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A rubber adhesive, characterized in that: It comprises the following components in parts by weight: 20-80 parts of hexamethoxymethylmelamine, 20-80 parts of white carbon black; The oil absorption value of the white carbon black is 1 to 5.4 cm 3 / g; The white carbon black is a highly dispersed white carbon black, and the highly dispersed white carbon black is a white carbon black whose dispersion degree in rubber reaches 9.5 or above.

2. The rubber adhesive according to claim 1, wherein The oil absorption value of the white carbon black is 4.4 cm 3 / g.

3. A rubber compound, characterized in that: include: Natural rubber, carbon black reinforcing agent, white carbon black, chemical additives, and adhesives; Wherein, the adhesive is the adhesive according to claim 1 or 2.

4. The rubber compound according to claim 3, characterized in that The invention comprises the following components by weight: 70 to 100 parts of natural rubber, 20 to 80 parts of carbon black reinforcing agent, 15 to 25 parts of white carbon black, 5 to 20 parts of chemical additives, and 1 to 10 parts of adhesive; The oil absorption value of the white carbon black in the rubber compound is 1 to 5.4 cm 3 / g, the white carbon black is highly dispersed white carbon black or ordinary white carbon black; The highly dispersed white carbon black is white carbon black with a dispersion degree of 9.5 or above in rubber; The ordinary white carbon black is white carbon black with a dispersion degree in rubber lower than grade 9.

5.

5. The rubber compound according to claim 3, characterized in that The chemical additives include at least two of an antioxidant, a vulcanizing agent, an accelerator and zinc oxide.

6. The rubber compound according to claim 5, characterized in that The antioxidant includes antioxidant RD and / or antioxidant 4020; And / or, the accelerator includes accelerator D and / or accelerator CZ; And / or, the vulcanizing agent is sulfur.

7. The rubber compound according to claim 5 or 6, characterized in that: The chemical auxiliary agent comprises the following components by weight: 1 to 3 parts of antioxidant, 1 to 3 parts of vulcanizing agent, 1.5 to 2 parts of accelerator and 5 to 10 parts of zinc oxide.

8. A method for preparing a rubber compound as claimed in any one of claim 7, characterized in that: The following steps are involved: The natural rubber is placed in an internal mixer and mixed to obtain plastic; The plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive are mixed in an internal mixer; then the material is discharged to an open mixer after the plug is pressed, and the material is turned over and cooled. After adding the vulcanizing agent and accelerator, the material is thinly passed, and the material is cooled to obtain a mixed rubber.

9. The method for preparing a rubber compound as claimed in claim 8, wherein: The natural rubber is placed in an internal mixer, the speed of the internal mixer is set to 30-55 rpm, the plug is pressed for 55-60 seconds, the plug is lifted and kept for 20-25 seconds, and then the plug is pressed to 160-165°C before discharging the material to obtain plastic; The plastic, zinc oxide, white carbon black, carbon black reinforcing agent, antioxidant and adhesive are placed in an internal mixer, and the speed of the internal mixer is set to 30-55 rpm. After pressing the bolt for 25-30 seconds, the bolt is lifted and held for 3-5 seconds, and then the bolt is pressed to 130-135°C and the bolt is lifted and held for 15-20 seconds; then the bolt is pressed to 150-155°C and then discharged to an open mixer, and the mixture is cooled to 90-100°C, and the vulcanizer and accelerator are added and thinned for 200-300 seconds, and the mixture is cooled to obtain a mixed rubber.