Method for improving smelting performance of vanadium-titanium sinter

By adding boron-containing additives to the vanadium-titanium powder sintered mixture, a low-melting ore phase was generated, which solved the problem of low-temperature reduction powdering performance and slag viscosity of the sintered ore after the vanadium-titanium powder ratio was improved, and the improvement of vanadium-titanium sintered ore was achieved. quality.

CN119082447APending Publication Date: 2024-12-06NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411255044.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the smelting and vanadium extraction process of vanadium titanium magnetite, the increase in the proportion of vanadium titanium powder leads to the deterioration of low-temperature reduction and slag sticking.

Method used

Boron-containing additives are added to the sintering mixture of vanadium-titanium powder, and sintered by rotating cloth to generate a low-melting ore phase, inhibit the formation of dicalcium silicate and reduce the liquid phase viscosity, and improve the low-temperature powderization index and slag viscosity of the sintered ore.

Benefits of technology

It effectively improves the low-temperature pulverization performance and slag viscosity of vanadium-titanium sintered ore, and improves the quality of sintered ore.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082447A_ABST
    Figure CN119082447A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the smelting performance of vanadium-titanium sinter, and relates to the technical field of blast furnace ironmaking. Comprising the following steps: S1, preparing a vanadium-titanium powder sintering mixture; s2, adding a boron-containing additive into the vanadium-titanium powder sintering mixture, and mixing and granulating; and S3, the mixture is put into a sintering cup for sintering in a rotary distribution mode. According to the method, the proportion of the vanadium-titanium powder in a sintered ore blending structure is 55% by adding the boron-containing additive, the content of the boron-containing additive is controlled to be 3%, the low-temperature pulverization index of the vanadium-titanium sintered ore can be improved to the maximum extent, and the slag viscosity can be reduced to the maximum extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of blast furnace ironmaking preparation, and in particular to a method for improving the smelting performance of vanadium-titanium sintered ore. Background Art

[0002] my country's vanadium-titanium magnetite is widely distributed and rich in reserves. Its reserves and mining volume rank third among China's iron mines. The proven reserves are nearly 10 billion tons, and the prospective reserves are more than 30 billion tons. Vanadium-titanium magnetite is a special iron ore resource. In addition to being rich in iron resources, it also contains valuable elements such as vanadium and titanium. In particular, vanadium is a scarce resource and a national strategic metal, known as the "MSG of modern industry." Therefore, vanadium-titanium ore is a mineral resource with great comprehensive utilization value.

[0003] At present, the vanadium extraction process is still mainly based on the blast furnace ironmaking-converter vanadium extraction-vanadium slag vanadium extraction process. However, due to the particularity of vanadium-titanium magnetite smelting and vanadium extraction process, when the proportion of vanadium-titanium powder in the ore matching structure is low, the vanadium content in the molten iron will be too low to be recovered, resulting in the loss of a large amount of vanadium resources. For this reason, the proportion of vanadium-titanium powder in the sintering ore matching structure should be increased. However, the particle size of vanadium-titanium powder is relatively fine. After increasing the proportion, it will affect the permeability of the sintering material layer. In addition, after the high proportion, the amount of liquid phase generated is reduced and the perovskite content is increased, resulting in poor low-temperature reduction pulverization performance and slag stickiness.

[0004] In view of the above problems, the present invention proposes a method for improving the sintering performance of vanadium titanium powder by adding a boron-containing additive. Summary of the invention

[0005] The purpose of the present invention is to provide a method for improving the smelting performance of vanadium-titanium sintered ore, so as to solve the problems mentioned in the above background technology that the low-temperature reduction pulverization performance of sintered ore deteriorates and the slag becomes sticky after increasing the ratio of vanadium-titanium powder.

[0006] To achieve the above object, the present invention provides a method for improving the smelting performance of vanadium-titanium sintered ore, comprising the following steps:

[0007] S1. preparing vanadium-titanium powder sintering mixture;

[0008] S2, adding a boron-containing additive to the vanadium-titanium powder sintering mixture, mixing and granulating;

[0009] S3. Place the mixed material into a sintering cup for sintering by means of a rotating distribution method.

[0010] Preferably, in S1, by mass percentage, 22.00% of 65% vanadium powder, 28.00% of 63.5% vanadium powder, 5.00% of Chilean coarse powder, 15.00% of general powder, 12.00% of PB, 11.00% of KR, 6.00% of miscellaneous materials and 1.00% of fluorine-containing fine powder are evenly mixed to obtain a sintered mixture with a vanadium-titanium powder 55% ore structure.

[0011] Preferably, the miscellaneous material is a mixture of 40% blast furnace gravity ash, 20% sintering machine head ash, and 40% environmental ash in percentage by mass.

[0012] Preferably, in S2, the boron-containing additive is boric acid.

[0013] Preferably, in S2, the mass percentage of boric acid is 0.5-7.5‰.

[0014] Preferably, in S3, the thickness of the sintering material layer is 700 mm.

[0015] Preferably, in S3, the sintering ignition negative pressure is 6.0 kPa, the ignition temperature is 1150±50° C., the ignition time is 80 seconds, and the sintering negative pressure is 10.0 kPa.

[0016] Preferably, in S3, the vertical sintering speed is 17.87-22.11 mm·min -1 .

[0017] Therefore, the present invention provides a method for improving the smelting performance of vanadium-titanium sintered ore. By adding a boron-containing additive into the sintering mixture, the boron-containing additive and the sintering mixture can easily generate a low-melting-point mineral phase, and can inhibit the formation of dicalcium silicate, and can reduce the viscosity of the liquid phase, improve the low-temperature pulverization index of the vanadium-titanium sintered ore and reduce the viscosity of the slag, thereby achieving the purpose of improving the quality of the vanadium-titanium sintered ore.

[0018] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the sintering process flow chart;

[0020] Figure 2 The figure is a result diagram of a soft melting dripping experiment on the sintered ores prepared in Examples 2, 3, 5 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0021] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, and simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.

[0022] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.

[0023] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0024] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.

[0025] Example 1

[0026] This embodiment provides a method for improving the smelting performance of vanadium-titanium sintered ore, comprising the following steps:

[0027] S1. Prepare a sintered mixture with a vanadium-titanium powder ore structure of 55% according to the material percentages in Table 1 below;

[0028] Table 1

[0029]

[0030]

[0031] S2, dissolving boric acid in water to obtain a boric acid solution with a mass percentage of 0.5‰, then pouring it into the sintering mixture and mixing it evenly, and performing secondary mixing and granulation;

[0032] S3. The mixed material is placed in a sintering cup for sintering by rotating the material distribution method. The sintering material layer thickness is 700 mm. The sintering ignition negative pressure is 6.0 kPa, the ignition temperature is 1150 ± 50 °C, the ignition time is 80 seconds, the sintering negative pressure is 10.0 kPa, and the vertical sintering speed is 20.33 mm min -1 .

[0033] Example 2

[0034] This embodiment provides a method for improving the smelting performance of vanadium-titanium sintered ore. The difference from Embodiment 1 is that in step S2, a boric acid solution with a mass percentage of 1‰ is used, and the vertical sintering speed in step S3 is 21.49 mm·min -1 The rest are the same as those in Example 1 and will not be repeated here.

[0035] Example 3

[0036] This embodiment provides a method for improving the smelting performance of vanadium-titanium sintered ore. The difference from Embodiment 1 is that in step S2, a boric acid solution with a mass percentage of 3‰ is used, and the vertical sintering speed in step S3 is 22.11 mm·min -1 The rest are the same as those in Example 1 and will not be repeated here.

[0037] Example 4

[0038] This embodiment provides a method for improving the smelting performance of vanadium-titanium sintered ore. The difference from Embodiment 1 is that in step S2, a boric acid solution with a mass percentage of 5‰ is used, and the vertical sintering speed in step S3 is 20.1 mm·min -1 The rest are the same as those in Example 1 and will not be repeated here.

[0039] Example 5

[0040] This embodiment provides a method for improving the smelting performance of vanadium-titanium sintered ore. The difference from Embodiment 1 is that in step S2, a boric acid solution with a mass percentage of 7.5‰ is used, and the vertical sintering speed in step S3 is 17.87 mm·min -1 The rest are the same as those in Example 1 and will not be repeated here.

[0041] Comparative Example 1

[0042] This comparative example provides a method for improving the smelting performance of vanadium-titanium sintered ore. The difference from Example 1 is that in step S2, no boric acid solution is added, and the vertical sintering speed in step S3 is 20.49 mm·min -1 The rest are the same as those in Example 1 and will not be repeated here.

[0043] Comparative Example 2

[0044] This comparative example provides a method for improving the smelting performance of vanadium-titanium sintered ore. The difference from Example 1 is that in step S2, a boric acid solution with a mass percentage of 15‰ is used, and the vertical sintering speed in step S3 is 18.5 mm·min -1 The rest are the same as those in Example 1 and will not be repeated here.

[0045] The products obtained after sintering in the above embodiments and comparative examples were cooled for ten minutes and poured into a container to measure the drum strength, low-temperature reduction pulverization performance and reduction performance of the sintered ore. Among them, the drum strength was measured according to the "Method for Determination of Drum Strength of Sintered Ore and Pellets" (YB / T5166-1993); the low-temperature reduction pulverization performance was measured according to the "Method for Using Cold Drums after Static Reduction of Iron Ore Low-Temperature Pulverization Test" (GB / T13242-2017); the reduction performance was measured according to the "Method for Determination of Reducibility of Iron Ore" (GB / T13241-2017).

[0046] The experimental results are shown in Table 2 below.

[0047] Table 2

[0048]

[0049]

[0050] From the data in Table 2, it can be seen that when the boric acid ratio varies between 1‰ and 3‰, the sintered ore yield and drum strength can meet the requirements of blast furnace production, and the low-temperature reduction pulverization performance is best when the boric acid ratio is 3‰.

[0051] The sintered ore prepared in Examples 2, 3, 5 and Comparative Example 1 was subjected to a soft melting dripping test. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that with the increase of boric acid content, the high melting point substances in the dripping slag gradually decrease, indicating that the addition of boric acid inhibits the precipitation of high melting point substances such as titanium nitride, titanium carbide and perovskite, and reduces the viscosity of the initial slag, so the dripping temperature decreases. This is because after the addition of boric acid, the content of solid-dissolved SiO2 in high melting point substances such as perovskite increases significantly, which reduces the melting point of high melting point substances such as perovskite, resulting in high melting point substances such as perovskite not being easy to crystallize during the cooling process and turning into glass. This is also the reason why the content of high melting point mineral phases such as perovskite in the slag decreases after increasing the boric acid content.

[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for improving the smelting performance of vanadium-titanium sintered ore, characterized in that: The following steps are involved: S1. preparing vanadium-titanium powder sintering mixture; S2, adding a boron-containing additive to the vanadium-titanium powder sintering mixture, mixing and granulating; S3. Place the mixed material into a sintering cup for sintering by means of a rotating distribution method.

2. A method for improving the smelting performance of vanadium-titanium sintered ore according to claim 1, characterized in that: In S1, the sintering mixture is composed of 22.00% of 65% vanadium powder, 28.00% of 63.5% vanadium powder, 5.00% of Chilean coarse powder, 15.00% of general powder, 12.00% of PB, 11.00% of KR, 6.00% of miscellaneous materials and 1.00% of fluorine-containing refined powder, which are uniformly mixed to obtain a sintering mixture with a vanadium-titanium powder 55% ore structure.

3. A method for improving the smelting performance of vanadium-titanium sintered ore according to claim 2, characterized in that: Calculated by mass percentage, the miscellaneous material is a mixture of 40% blast furnace gravity ash, 20% sintering machine head ash, and 40% environmental ash.

4. The method for improving the smelting performance of vanadium-titanium sintered ore according to claim 1, characterized in that: In the S2, the boron-containing additive is boric acid.

5. The method for improving the smelting performance of vanadium-titanium sintered ore according to claim 1, characterized in that: In the S2, the mass percentage of the boron-containing additive is 0.5 to 7.5‰.

6. The method for improving the smelting performance of vanadium-titanium sintered ore according to claim 1, characterized in that: In the S3, the thickness of the sintering material layer is 700 mm.

7. The method for improving the smelting performance of vanadium-titanium sintered ore according to claim 1, characterized in that: In S3, the sintering ignition negative pressure is 6.0 kPa, the ignition temperature is 1150±50° C., the ignition time is 80 seconds, and the sintering negative pressure is 10.0 kPa.

8. The method for improving the smelting performance of vanadium-titanium sintered ore according to claim 1, characterized in that: In S3, the vertical sintering speed is 17.87-22.11 mm·min -1 .

Citation Information

Patent Citations

  • Sintering method for high-titanium type vanadium titanium magnet concentrate with added boride

    CN102242256A

  • Preparation method of high-ferrum low-silicon vanadium-titanium sintering ore

    CN102758084A

  • Novel blast furnace comprehensive furnace burden structure based on MgO partition

    CN112481431A

  • Vanadium-titanium sintered ore preparation method under high pellet proportion smelting condition

    CN115125389A

  • Production method of boron-containing vanadium-titanium sintered ore

    CN117127009A