Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst as well as preparation method and application thereof

The preparation of Fe2Ni5 crystal-amorphous heterostructure aerogel catalyst by wet chemical co-precipitation method has solved the problems of complex preparation of aerogel catalysts and poor OER performance in the prior art, and achieved efficient electrolytic oxygen analysis performance. Improves the efficiency of hydrogen production by electrolyzing water.

CN119082766APending Publication Date: 2024-12-06CHENGDU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411212279.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing aerogel catalyst preparation process is complex and costly, and it is difficult to produce industrially. The OER performance of transition metal catalysts is not ideal, especially in electrolytic water reactions, with greater kinetic resistance.

Method used

The Fe2Ni5 crystal-amorphous heterostructure aerogel catalyst was prepared by wet chemical co-precipitation method. FeNi3 crystal clusters were grown inside the amorphous gel particles of iron-nickel hydroxide by mild reducing properties of dimethylammonium borane. A heterogeneous catalytically active site with a crystal-amorphous heterostructure is formed.

Benefits of technology

It realizes efficient oxygen analysis performance of electrolytic water, significantly improves the efficiency of hydrogen production of electrolytic water, and provides a simple and safe industrial preparation solution with excellent catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082766A_ABST
    Figure CN119082766A_ABST
Patent Text Reader

Abstract

The invention discloses a Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst as well as a preparation method and application thereof, and belongs to the technical field of catalysts. The transition metal aerogel material is prepared through a wet chemical coprecipitation method, by means of the mild reduction property of dimethylamine borane, FeNi3 crystal form clusters slowly grow in iron-nickel hydroxide amorphous colloidal particles, heterogeneous catalytic active sites with a crystal-amorphous (c-a) heterostructure are generated, and the transition metal aerogel material is prepared. And generating a mixed tissue material of an aerogel three-dimensional structure and a (c-a) heterostructure. The prepared Fe2Ni5 type crystal-amorphous heterostructure aerogel catalyst has excellent water electrolysis oxygen evolution performance, and the water electrolysis hydrogen production efficiency can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst and a preparation method and application thereof. Background Art

[0002] Energy issues are currently a major problem that hinders human development. It is urgent to seek a green, environmentally friendly, sustainable, efficient and cheap new energy source. Hydrogen energy, as the cleanest and renewable new energy source, is a substitute for fossil fuels in the future. The use of renewable energy such as solar energy for water electrolysis is considered to be the most promising method for the preparation of "green hydrogen". However, it is necessary to overcome a large kinetic resistance in the water electrolysis reaction. This is because in actual production, the oxygen evolution reaction (OER) at the anode in the overall water splitting reaction involves four electron transfer processes. Therefore, the preparation of OER catalysts with good catalytic performance is the key to improving the efficiency of hydrogen production by water electrolysis.

[0003] Early studies found that precious metal materials such as platinum-based / ruthenium-based / iridium-based materials exhibited superior catalytic performance, but their high prices seriously hindered their application in OER. Transition metals have attracted extensive research due to their excellent catalytic performance, abundant reserves and low prices, but the catalytic effect of transition metals alone is not ideal. In recent years, researchers have found that the synergistic effect between transition metals can effectively reduce the free energy of OER reactions and thereby prepare many excellent catalysts, such as transition metal alloys, transition metal hydroxides, and transition metal oxides.

[0004] The large number of unsaturated sites and flexible self-driven structures inside the structure of amorphous materials can quickly reconstruct themselves during the OER reaction to meet the reaction requirements. Studies have shown that the catalytic ability of amorphous catalysts is better than that of crystalline catalysts, but due to the irregular arrangement of atoms, their conductivity is often low. Aerogels provide more active sites for OER reactions due to their unique high porosity and self-supporting three-dimensional framework structure, and their cross-connected three-dimensional network greatly accelerates electron transfer, which makes aerogels exhibit superior catalytic performance in the field of OER. However, most current research focuses on precious metal aerogels or carbon-based aerogels with complex synthesis processes loaded with non-precious metals. This process of making aerogels is slow and complicated, which is not conducive to industrial hydrogen production. If the amorphous structure is organically combined with the aerogel structure, the metal atoms are automatically assembled to form an aerogel skeleton through wet chemical reduction, and pure transition metal aerogels with controllable composition, morphology, performance, high specific surface area and high porosity are prepared. In addition, a large number of studies have shown that a compact crystalline-amorphous (ca) heterostructure can provide more reactive sites and greater reaction driving force for the migration of electrons. These characteristics give the crystalline-amorphous (ca) heterostructure a unique advantage in the field of catalysts. Therefore, if a pure transition metal aerogel with a distinct crystalline and amorphous structure can be produced using a simple synthesis method and relatively safe industrial raw materials, it will provide a new solution for the preparation of transition metal catalysts.

[0005] In the field of aerogel catalyst preparation, hydrogels are currently mainly prepared by hydrothermal and sol-gel methods, and then aerogels are obtained by environmental drying, freeze drying or supercritical drying. Among them, the hydrothermal method creates a high-temperature, high-pressure reaction environment by heating the reaction vessel. As the reaction proceeds, the partially reduced GO sheets gradually self-assemble into a three-dimensional network structure through π-π interactions and van der Waals forces to form a hydrogel. At the same time, N elements and ruthenium elements are loaded onto the aerogel during the graphene hydrogel generation process, and finally a precious metal-loaded graphene hydrogel with a core-shell structure is formed. Graphene aerogels are subsequently prepared by freeze drying. The sol-gel method usually dissolves metal organic or inorganic precursors (such as metal alkoxides, chlorides, etc.) in a solvent, and generates metal hydroxyl complexes through hydrolysis reactions, and then generates MOM (M represents metal) bonds through condensation reactions to form sol particles, and finally obtains aerogels through supercritical CO2 drying. The preparation process of carbon-based aerogels by hydrothermal method is complicated and often requires the synthesis of multiple precursors. After obtaining the aerogel, it is also necessary to grow metal crystals by heat treatment. The preparation of aerogels by sol-gel method often requires precise control of multiple steps in the preparation process, and finally, repeated washing is usually required to remove residual condensing agents in the preparation process. The above two methods of preparing aerogels have more process control links and higher costs, which are not conducive to industrial-scale production. In addition, the growth environment of the sol-gel method is relatively harsh, and it is difficult to promote in actual production.

[0006] In the preparation process of transition metal crystalline-amorphous (CA) heterostructures, the current common preparation method is to first prepare a material with a crystalline structure, then prepare a material with an amorphous structure, and finally prepare a crystalline-amorphous (CA) heterostructure by hydrothermal or electrodeposition. This method is not only cumbersome, but also difficult to synthesize metal nanoparticles with a compact crystalline-amorphous (CA) heterostructure, which will result in a loose bond between the crystalline and amorphous interfaces, increase the resistance to charge transfer, and reduce the OER performance of the catalyst. Summary of the invention

[0007] In view of the above-mentioned prior art, the present invention provides a Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst and a preparation method and application thereof, so as to solve the technical problems that the existing aerogel catalyst is difficult to prepare and has poor hydrogen evolution catalytic performance.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is to provide a method for preparing a Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst, comprising the following steps:

[0009] S1: dissolving ferric chloride hexahydrate and nickel chloride hexahydrate in water to obtain an aqueous solution of iron-nickel metal salts; dissolving dimethylamine borane in water to obtain an aqueous solution of dimethylamine borane;

[0010] S2: adding the aqueous solution of dimethylamine borane to the iron-nickel metal salt solution, mixing well, and obtaining a mixed solution;

[0011] S3: adding potassium hydroxide to the mixed solution and mixing well to obtain a nickel iron hydroxide colloidal solution;

[0012] S4: incubating the iron-nickel hydroxide colloidal solution at 20-30° C. in the dark for 45-50 h to obtain a Fe2Ni5 type iron-nickel based hydrogel;

[0013] S5: Wash the Fe2Ni5 type iron-nickel based hydrogel with deionized water for 2 to 4 times, and then freeze-dry it to obtain.

[0014] Based on the above technical solution, the present invention can also be improved as follows.

[0015] Furthermore, the molar ratio of ferric chloride hexahydrate to nickel chloride hexahydrate in the iron-nickel metal salt aqueous solution is 2:5.

[0016] Furthermore, the molar ratio of dimethylamine borane to nickel chloride hexahydrate in the mixed solution is 1:100.

[0017] Further, the molar ratio of the added amount of potassium hydroxide to the nickel chloride hexahydrate is 1:1.

[0018] Furthermore, the incubation temperature in S4 is 25° C., and the incubation time is 48 h.

[0019] Furthermore, the deionized water cleaning in S5 includes the following steps: immersing the Fe2Ni5 type iron-nickel based hydrogel in deionized water and centrifuging at a speed of 8000 rpm for 10 to 20 minutes.

[0020] Furthermore, the freeze-drying temperature in S5 is -40 to -20°C, and the drying time is 10 to 15 hours.

[0021] The invention also discloses a Fe2Ni5 type crystal-amorphous heterostructure aerogel catalyst prepared by the preparation method.

[0022] The invention also discloses the application of the Fe2Ni5 type crystal-amorphous heterostructure aerogel catalyst in hydrogen production by water electrolysis.

[0023] The beneficial effects of the present invention are:

[0024] The present invention realizes the preparation of transition metal aerogel materials by wet chemical coprecipitation method, and utilizes the mild reducing property of dimethylaminoborane to slowly grow FeNi3 crystal clusters inside the amorphous colloid particles of iron nickel hydroxide, generate multiphase catalytic active sites with crystal-amorphous (ca) heterostructure, and generate aerogel three-dimensional structure and (ca) heterostructure mixed tissue material. The prepared Fe2Ni5 type crystal-amorphous heterostructure aerogel catalyst has excellent electrolytic water oxygen evolution performance and can effectively improve the efficiency of electrolytic water hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the SEM photo of the Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst;

[0026] Figure 2 This is the TEM photo of Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst;

[0027] Figure 3 The XRD diffraction pattern of Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst;

[0028] Figure 4 LSV curve of the OER performance of Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst. DETAILED DESCRIPTION

[0029] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0030] Example 1

[0031] A Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst is prepared by the following steps:

[0032] S1: Dissolve 2 mmol of ferric chloride hexahydrate in 50 mL of water to obtain a ferric chloride solution; dissolve 5 mmol of nickel chloride hexahydrate in 50 mL of water to obtain a nickel chloride solution; pour the ferric chloride solution and the nickel chloride solution into 50 mL of deionized water, stir evenly, and obtain an iron-nickel metal salt aqueous solution.

[0033] S2: In a water bath at 30°C, 0.5 mol of dimethylamine borane is dissolved in 100 mL of water by stirring to obtain a dimethylamine borane solution; immediately after the stirring, the dimethylamine borane solution is added to the prepared iron-nickel metal salt solution to obtain a mixed solution; no stirring is required during the mixing process;

[0034] S3: adding 5 ml of 1 M KOH solution to the mixed solution in five times, 1 ml each time, without stirring during the addition; after the addition is completed, a nickel iron hydroxide colloidal solution is obtained;

[0035] S4: The iron-nickel hydroxide colloidal solution is sealed and incubated in a dark environment for 48 hours at a temperature of 25° C. to obtain a Fe2Ni5 type iron-nickel based hydrogel;

[0036] S5: Place the Fe2Ni5 type iron-nickel based hydrogel into a 50 mL centrifuge tube, add deionized water to submerge the hydrogel, and then centrifuge at 8000 rpm for 15 min. After the centrifugation is completed, clean up the deionized water; repeat the above operation twice;

[0037] S6: The cleaned Fe2Ni5 iron-nickel based hydrogel is placed in a freeze dryer and dried at -30°C for 12 hours to obtain a Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst.

[0038] Example 2

[0039] A Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst is prepared by the following steps:

[0040] S1: Dissolve 2 mmol of ferric chloride hexahydrate in 50 mL of water to obtain a ferric chloride solution; dissolve 5 mmol of nickel chloride hexahydrate in 50 mL of water to obtain a nickel chloride solution; pour the ferric chloride solution and the nickel chloride solution into 50 mL of deionized water, stir evenly, and obtain an iron-nickel metal salt aqueous solution.

[0041] S2: In a water bath at 30°C, 0.5 mol of dimethylamine borane is dissolved in 100 mL of water by stirring to obtain a dimethylamine borane solution; immediately after the stirring, the dimethylamine borane solution is added to the prepared iron-nickel metal salt solution to obtain a mixed solution; no stirring is required during the mixing process;

[0042] S3: adding 5 ml of 1 M KOH solution to the mixed solution in five times, 1 ml each time, without stirring during the addition; after the addition is completed, a nickel iron hydroxide colloidal solution is obtained;

[0043] S4: The iron-nickel hydroxide colloidal solution is sealed and incubated in a dark environment for 45 hours at a temperature of 30° C. to obtain a Fe2Ni5 type iron-nickel based hydrogel;

[0044] S5: Place the Fe2Ni5 type iron-nickel based hydrogel into a 50 mL centrifuge tube, add deionized water to submerge the hydrogel, and then centrifuge at 8000 rpm for 10 min. After the centrifugation is completed, clean up the deionized water; repeat the above operation twice;

[0045] S6: The cleaned Fe2Ni5 iron-nickel based hydrogel is placed in a freeze dryer and dried at -40°C for 10 hours to obtain a Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst.

[0046] Example 3

[0047] A Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst is prepared by the following steps:

[0048] S1: Dissolve 2 mmol of ferric chloride hexahydrate in 50 mL of water to obtain a ferric chloride solution; dissolve 5 mmol of nickel chloride hexahydrate in 50 mL of water to obtain a nickel chloride solution; pour the ferric chloride solution and the nickel chloride solution into 50 mL of deionized water, stir evenly, and obtain an iron-nickel metal salt aqueous solution.

[0049] S2: In a water bath at 30°C, 0.5 mol of dimethylamine borane is dissolved in 100 mL of water by stirring to obtain a dimethylamine borane solution; immediately after the stirring, the dimethylamine borane solution is added to the prepared iron-nickel metal salt solution to obtain a mixed solution; no stirring is required during the mixing process;

[0050] S3: adding 5 ml of 1 M KOH solution to the mixed solution in five times, 1 ml each time, without stirring during the addition; after the addition is completed, a nickel iron hydroxide colloidal solution is obtained;

[0051] S4: The iron-nickel hydroxide colloidal solution is sealed and incubated in a dark environment for 50 hours at a temperature of 20° C. to obtain a Fe2Ni5 type iron-nickel based hydrogel;

[0052] S5: Place the Fe2Ni5 type iron-nickel based hydrogel into a 50 mL centrifuge tube, add deionized water to submerge the hydrogel, and then centrifuge at 8000 rpm for 20 min. After the centrifugation is completed, clean up the deionized water; repeat the above operation twice;

[0053] S6: The cleaned Fe2Ni5 iron-nickel based hydrogel is placed in a freeze dryer and dried at -20°C for 15 hours to obtain a Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst.

[0054] Results Analysis

[0055] The Fe2Ni5 type crystal-amorphous heterostructure aerogel catalysts prepared in Examples 1 to 3 of the present invention have similar performances. Taking the Fe2Ni5 type crystal-amorphous heterostructure aerogel catalyst in Example 1 as an example, its performance is described.

[0056] The morphology of the Fe2Ni5 type crystal-amorphous heterostructure aerogel catalyst in the present invention was tested, and the results are as follows: Figures 1 to 3 As shown; among them, Figure 1 This is the SEM test result. Figure 2 This is the TEM test result. Figure 3 The XRD test results are as follows. Figures 1 to 3 It can be seen that Figure 1It shows that the Fe2Ni5 type crystal-amorphous heterostructure aerogel presents a porous three-dimensional structure. Figure 2 It shows that there are a lot of amorphous tissues and a small amount of crystalline tissues in the Fe2Ni5 type crystal-amorphous heterostructure aerogel, in which the crystalline tissues exist in the form of nanoclusters and are tightly wrapped by the amorphous tissues. Figure 3 It shows that the amorphous structure is the main body in the Fe2Ni5 type crystal-amorphous heterostructure aerogel structure.

[0057] The OER performance of the Fe2Ni5 type crystalline-amorphous heterostructure aerogel catalyst in the present invention was tested using a typical three-electrode test system. Figure 4 As shown in the test, it was found that the Fe2Ni5 type crystalline-amorphous heterostructure aerogel was -2 At this current density, the overpotential is 262mV.

[0058] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A kind of Fe 2 Ni 5 Preparation method of crystalline-amorphous heterostructure aerogel catalyst, It is characterized in that The following steps are involved: S1: dissolving ferric chloride hexahydrate and nickel chloride hexahydrate in water to obtain an aqueous solution of iron-nickel metal salts; dissolving dimethylamine borane in water to obtain an aqueous solution of dimethylamine borane; S2: adding the aqueous solution of dimethylamine borane to the iron-nickel metal salt solution, mixing well, and obtaining a mixed solution; S3: adding potassium hydroxide to the mixed solution and mixing well to obtain a nickel iron hydroxide colloidal solution; S4: Incubate the nickel iron hydroxide colloidal solution at 20-30°C in the dark for 45-50h to obtain Fe 2 Ni 5 Type iron-nickel based hydrogel; S5: Wash Fe with deionized water 2 Ni 5 The type iron-nickel based hydrogel is prepared 2 to 4 times and then freeze-dried to obtain the hydrogel.

2. The preparation method according to claim 1, Features: The molar ratio of ferric chloride hexahydrate to nickel chloride hexahydrate in the iron-nickel metal salt aqueous solution is 2:

5.

3. The preparation method according to claim 1, Features: The molar ratio of dimethylamine borane to nickel chloride hexahydrate in the mixed solution is 1:

100.

4. The preparation method according to claim 1, Features: The molar ratio of the added amount of potassium hydroxide to the nickel chloride hexahydrate is 1:

1.

5. The preparation method according to claim 1, Features: The incubation temperature in S4 was 25°C and the incubation time was 48 h.

6. The preparation method according to claim 1, It is characterized in that The deionized water cleaning in S5 includes the following steps: 2 Ni 5 The iron-nickel based hydrogel was immersed in deionized water and centrifuged at 8000 rpm for 10 to 20 min.

7. The preparation method according to claim 1, Features: The freeze drying temperature in S5 is -40 to -20°C, and the drying time is 10 to 15 hours.

8. Fe prepared by the preparation method according to any one of claims 1 to 7 2 Ni 5 Crystal-amorphous heterostructure aerogel catalyst.

9. Fe according to claim 8 2 Ni 5 Application of crystalline-amorphous heterostructure aerogel catalysts in hydrogen production by water electrolysis.

Citation Information

Cited By

  • Aerogel catalyst with core-shell structure as well as preparation method and application of aerogel catalyst

    CN119346119A