Additive, electrolyte, rechargeable lithium battery, and method of manufacturing same

By using the additives represented by Chemical Formula 1 in the rechargeable lithium battery, a stable SEI film is formed, which solves the problems of increased resistance and reduced cycle life, and significantly improves the high-temperature storage and room temperature operation performance of lithium batteries.

CN119092821APending Publication Date: 2024-12-06SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410714138.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-05
Filing Date
2024-06-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Rechargeable lithium batteries are prone to increased resistance and reduced cycle life when operating at room temperature and high temperatures, especially when cobalt-free positive electrode active substances and high-temperature storage conditions.

Method used

Using the additive represented by Chemical Formula 1, the additive is composed of a compound of two anhydride structures connected by an aliphatic or aromatic ring, which can form a stable solid electrolyte interface (SEI) film on the surface of the negative electrode, inhibiting the increase in resistance and improving cycle life. characteristic.

Benefits of technology

It effectively suppresses the increase in resistance of rechargeable lithium batteries at room temperature and high temperatures, extends the cycle life, and maintains the performance of the battery under high temperature storage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092821A_ABST
    Figure CN119092821A_ABST
Patent Text Reader

Abstract

The present application provides an additive for use in an electrolyte of a rechargeable lithium battery, an electrolyte including the additive, a rechargeable lithium battery including the electrolyte, and a method of manufacturing the rechargeable lithium battery. The additive is a compound having two anhydride functional groups linked by an aliphatic ring or an aromatic ring.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] According to one or more embodiments, the present disclosure relates to an additive, an electrolyte for a rechargeable lithium battery including the additive, a rechargeable lithium battery, and a method of manufacturing the rechargeable lithium battery. Background Art

[0002] The rechargeable lithium battery is rechargeable and has a high energy density per unit weight of up to three times or more compared to comparable lead-acid batteries, nickel-cadmium batteries, nickel-metal hydride batteries, nickel-zinc batteries, etc. It can also be charged at a high rate, and therefore, is commercially manufactured for use in laptop computers, cellular phones, power tools, electric bicycles, etc., and research on improving additional energy density has been actively conducted or sought.

[0003] A rechargeable lithium battery may be realized by injecting an electrolyte into an electrode assembly including a positive electrode (eg, including a positive electrode active material) and a negative electrode (eg, including a negative electrode active material).

[0004] One of the latest developments in the technology for rechargeable lithium batteries is to improve (or provide appropriate) high temperature charge / discharge and storage characteristics, and to improve (or provide appropriate) room temperature charge / discharge characteristics. In general, rechargeable lithium batteries may experience increased resistance and / or decreased cycle life after repeated charging and discharging at room temperature. These undesirable changes may become more severe if (for example, when) a positive electrode active material that does not contain cobalt is used and / or the rechargeable lithium battery is stored at relatively high temperatures. Summary of the invention

[0005] One or more aspects relate to an additive for an electrolyte of a rechargeable lithium battery, which improves cycle-life characteristics while suppressing or reducing an increase in resistance of the rechargeable lithium battery at room temperature and / or high temperature.

[0006] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the presented embodiments of the disclosure.

[0007] An additive for an electrolyte for a rechargeable lithium battery according to one or more embodiments may be represented by Chemical Formula 1:

[0008] Chemical formula 1

[0009]

[0010] In Chemical Formula 1,

[0011] A may be a substituted or unsubstituted C3-C10 aliphatic ring or a substituted or unsubstituted C6-C20 aromatic ring; and

[0012] X 1 and X 2 can be O or S independently.

[0013] The additive according to some embodiments may form a stable solid electrolyte interface (SEI) film on the surface of the negative electrode, thereby suppressing or reducing resistance increase during operation of a rechargeable lithium battery at room temperature and / or high temperature and improving cycle-life characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 to Figure 3 is a schematic diagram illustrating a rechargeable lithium battery according to some embodiments.

[0015] Reference numerals

[0016] 100: Rechargeable lithium battery

[0017] 10: Positive electrode

[0018] 20: Negative electrode

[0019] 30: Diaphragm

[0020] 40: Electrode assembly

[0021] 50: Shell

[0022] 60: Sealing component

[0023] 70: Electrode terminal DETAILED DESCRIPTION

[0024] Hereinafter, rechargeable lithium batteries according to some embodiments will be described in more detail with reference to the accompanying drawings so that those of ordinary skill in the art can easily implement them. Examples thereof are illustrated in the accompanying drawings, in which the same reference numerals refer to the same elements throughout, and a repeated description thereof may not be provided. Accordingly, embodiments are described with reference to the accompanying drawings to explain aspects of this specification. However, these embodiments are only examples, and the disclosure is not limited thereto. On the contrary, the disclosure may be embodied in many different forms and is limited by the scope of the claims.

[0025] The terms used herein are for describing embodiments only and are not intended to limit the present disclosure. The singular expressions "a," "an," and "the" include plural expressions (including "at least one") unless the context clearly indicates otherwise.

[0026] As used herein, "combinations thereof" refers to mixtures, laminates, composites, copolymers, alloys, blends, reaction products, and the like of components.

[0027] In this document, it should be understood that terms such as “comprises,” “comprise,” “comprising,” “includes,” “including,” “include,” “having,” “has,” and / or “have” are intended to mark the existence of specified aspects, quantities, operations, elements, and / or combinations thereof (e.g., any appropriate combination), but do not exclude the possibility of the existence or addition of one or more other features, quantities, operations, elements, and / or combinations thereof (e.g., any appropriate combination).

[0028] In the accompanying drawings, the thickness of layers, films, panels, regions, etc. are exaggerated for clarity, wherein the same reference numerals represent the same elements, and a repeated description thereof may not be provided throughout the specification. It will be understood that if (for example, when) an element (such as a layer, film, region, or substrate) is referred to as being "on" another element (such as a layer, film, region, or substrate), it may be directly on the other element (such as a layer, film, region, or substrate), or there may also be intervening elements. In contrast, if (for example, when) an element (such as a layer, film, region, or substrate) is referred to as being "directly on" another element (such as a layer, film, region, or substrate), there are no intervening elements.

[0029] In one or more embodiments, the term “layer” herein includes not only a shape formed on the entire surface but also a shape formed on a partial surface if (for example, when) viewed from a plan view.

[0030] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe one or more appropriate elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings described herein, the first element, component, region, layer or part described herein may be referred to as a second element, component, region, layer or part.

[0031] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. Expressions such as "at least one of," "one of," and "selected from," if (e.g., when) preceding / following a list of elements, modify the entire list of elements and do not modify the individual elements of the list. For example, the expressions "at least one of a to c" and "at least one of a, b, and c" may indicate only a, only b, only c, both a and b (e.g., simultaneously), both a and c (e.g., simultaneously), b and c (e.g., simultaneously), all of a, b, and c, or variations thereof.

[0032] Spatially relative terms such as "below," "below," "below," "above," "on," etc. may be used herein to easily describe the relationship of one element or feature to another element or feature. It will be understood that the spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientations illustrated in the drawings. For example, if (e.g., when) the device in the drawings is turned over, an element described as being "below" or "below" other elements or features will be oriented "above" the other elements or features. Thus, the example term "below" may (e.g., simultaneously) encompass both the orientations above and below. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative terms used herein may be interpreted accordingly.

[0033] The terms used in this article are only used for the purpose of describing a particular embodiment and are not intended to limit the present disclosure. Unless otherwise defined, all terms used in the present disclosure (including chemical, technical and scientific terms) are the same as those commonly understood by those of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with the meaning in the context of the relevant field and the present disclosure, and will not be interpreted in an ideal or overly formal sense.

[0034] Example embodiments are described herein with reference to cross-sectional views of schematic diagrams as ideal embodiments. As such, variations in the shapes illustrated can be expected due to, for example, manufacturing techniques and / or tolerances. Therefore, the embodiments described herein should not be construed as limited to the specific shapes of the zones illustrated herein, but rather include deviations in shape, for example, caused by manufacturing. For example, a zone illustrated or described as flat may typically have rough and / or nonlinear features. Moreover, illustrated sharp angles may be rounded. Therefore, the zones illustrated in the accompanying drawings are schematic in nature, and their shapes are not intended to illustrate the precise shape of the zones, and are not intended to limit the scope of the claims.

[0035] The term "may" will be understood to refer to "one or more embodiments of the present disclosure," some of which include the described elements and some of which do not include the elements and / or include alternative elements. Similarly, optional language such as "or" refers to "one or more embodiments of the present disclosure" that each include the corresponding listed items.

[0036] In this context, "consisting essentially of" means that any additional components do not significantly affect the chemical, physical, optical or electrical properties of the target moiety.

[0037] Further, in this specification, the phrase "on a plane" or "plan view" means observing a target portion from the top, and the phrase "in a cross section" means observing a cross section formed by vertically cutting the target portion from the side.

[0038] definition

[0039] The term "particle size" as used herein refers to the average diameter of the particles if (e.g., when) the particles are spherical, and refers to the average major axis length of the particles if (e.g., when) the particles are non-spherical. For example, the average particle size can be measured by a method well suited to those skilled in the art, for example, by a particle size analyzer, or by a transmission electron microscope image or a scanning electron microscope image. The average particle size value can be obtained by measuring using a dynamic light scattering method, performing data analysis, calculating the number of particles in each particle size range and calculating therefrom. Unless otherwise specified, the average particle size (D 50 ) may refer to the diameter of particles whose cumulative volume is 50% by volume in a particle size distribution. If (for example, when) measurement is performed by laser diffraction, more specifically, the particles to be measured are dispersed in a dispersion medium, and then introduced into a laser diffraction particle size measuring device of the related art (for example, MT 3000 available from Microtrac, Ltd.) using ultrasonic waves of about 28 kHz, and after irradiation at an output of 60 W, the average particle diameter (D ) based on 50% of the particle size distribution in the measuring device can be calculated. 50 As used herein, if (for example, when) a definition is provided otherwise, the average particle size (D 50 ) refers to the diameter of particles accounting for 50% by volume of the cumulative volume in a particle size distribution obtained by randomly measuring the sizes (diameters or major axis lengths) of about 20 particles in a scanning electron microscope image.

[0040] In the present disclosure, "does not include one or any 'component'", "excludes one or any 'component'", "does not contain 'component'", etc. means that the 'component' is not added, selected or used as a component in the composition / structure, but due to other impurities and / or external factors, less than an appropriate amount of the 'component' may still be included.

[0041] In this document, “or” is not interpreted as being exclusive. For example, “A or B” is interpreted as including A, B, A+B, etc.

[0042] The term "metal" is interpreted as a concept including common metals, transition metals, and metalloids (semimetals).

[0043] As used herein, "substituted" means that at least one hydrogen of a compound is replaced by a substituent selected from the group consisting of a halogen atom (F, Cl, Br or I), a hydroxyl group, a C1-C20 alkoxy group, a nitro group, a cyano group, an amine group, an imino group, an azido group, an amidine group, a hydrazine group, a hydrazone group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, an ether group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, a C1-C20 alkyl group, a C2-C20 alkenyl group, a C2-C20 alkynyl group, a C6-C20 aryl group, a C3-C20 cycloalkyl group, a C3-C20 cycloalkenyl group, a C3-C20 cycloalkynyl group, a C2-C20 heterocycloalkyl group, a C2-C20 heterocycloalkenyl group, a C2-C20 heterocycloalkynyl group, a C3-C20 heteroaryl group and / or combinations thereof (e.g., any appropriate combination).

[0044] Herein, for example, C1-C20 means having 1 to 20 carbon atoms.

[0045] additive

[0046] Some embodiments provide an additive for an electrolyte of a rechargeable lithium battery represented by Chemical Formula 1:

[0047] Chemical formula 1

[0048]

[0049] In Chemical Formula 1, A may be a substituted or unsubstituted C3-C10 aliphatic ring or a substituted or unsubstituted C6-C20 aromatic ring; and X 1 and X 2 can be O or S independently.

[0050] The additive of some embodiments may be a compound having a structure of two anhydrides connected by an aliphatic ring or an aromatic ring (chemical formula 1). Herein, the compound having a structure of two anhydrides connected by an aliphatic ring or an aromatic ring (chemical formula 1) may be reduced and / or decomposed on the negative electrode surface during operation of the rechargeable lithium battery, for example, to form (provide) a stable solid electrolyte interface (SEI) film. The stable SEI film formed on the negative electrode surface can improve cycle life characteristics and suppress or reduce the resistance increase during operation of the rechargeable lithium battery at room temperature and / or high temperature.

[0051] A description of Chemical Formula 1 representing the additive is as follows.

[0052] A may be a cyclohexane ring or a benzene ring.

[0053] X 1 and X 2 Can both (for example, simultaneously) be 0.

[0054] Representative examples of the additive represented by Chemical Formula 1 may include the following Chemical Formula 1-1 and Chemical Formula 1-2:

[0055] Chemical formula 1-1

[0056]

[0057] Chemical formula 1-2

[0058]

[0059] Electrolytes

[0060] Some embodiments provide an electrolyte for a rechargeable lithium battery, the electrolyte including: a non-aqueous organic solvent; a lithium salt; and an additive represented by Chemical Formula 1.

[0061] Chemical formula 1

[0062]

[0063] Description of additives is as described herein.

[0064] The electrolyte of some embodiments may form (or provide) a stable SEI (solid electrolyte interface) film on the negative electrode surface through the additive, and thereby improve cycle life characteristics, and suppress or reduce resistance increase during operation of the rechargeable lithium battery at room temperature and / or high temperature.

[0065] The description of the additives is the same as described in the aforementioned one or more embodiments.

[0066] Content of additives

[0067] Based on 100 wt % of the electrolyte, the additive may be included in an amount of about 0.05 to about 3.0 wt %, 0.5 to about 3.0 wt %, about 0.05 to about 2 wt % or about 0.05 to about 1 wt %. Within the described range, the compound having a structure of two acid anhydrides connected by an aliphatic ring or an aromatic ring (Chemical Formula 1) may be reduced and decomposed on the negative electrode surface, and thus form (or provide) a stable SEI film.

[0068] Non-aqueous organic solvents

[0069] The non-aqueous organic solvent is used as a medium for transporting ions participating in the electrochemical reaction of the battery. For example, the non-aqueous organic solvent can be a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent, an aprotic solvent and / or a combination thereof (for example, any appropriate combination).

[0070] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethylmethyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, decanoic acid lactone, mevalonolactone, valerolactone, caprolactone, etc.

[0071] Ether solvents may include dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. Ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc., and aprotic solvents may include nitriles (such as R-CN, where R is a C2-C20 straight chain hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group, and may include a double bond, an aromatic ring, or an ether group), amides (such as dimethylformamide), dioxolanes (such as 1,3-dioxolanes or 1,4-dioxolanes), sulfolane, etc.

[0072] The non-aqueous organic solvent can be used alone or as (e.g., among them) two or more combinations. If (e.g., when) used in two or more combinations, the mixing ratio can be suitably adjusted according to the desired or appropriate battery performance, which is well known to those skilled in the art.

[0073] In addition, if (for example, when) a carbonate-based solvent is used, a cyclic carbonate and a chain carbonate may be mixed and used. For example, the cyclic carbonate and the chain carbonate may be mixed in a volume ratio of about 1:1 to about 1:9.

[0074] The non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent. For example, a carbonate-based solvent and an aromatic hydrocarbon organic solvent may be mixed and used in a volume ratio of about 1:1 to about 30:1.

[0075] The electrolyte may further include vinyl ethylene carbonate, vinylene carbonate, or ethylene carbonate-based compounds, for example, to improve battery cycle life.

[0076] Representative examples of the ethylene carbonate-based compound may include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.

[0077] Lithium salts

[0078] The lithium salt dissolved in the non-aqueous organic solvent supplies lithium ions in the battery, ensures the basic operation of the rechargeable lithium battery, and improves the transfer of lithium ions between the positive electrode and the negative electrode. Examples of lithium salts may include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide, LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are integers of 1 to 20), at least one (e.g., one or more) of lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalato)phosphate (LiDFOB), and lithium bis(oxalato)borate (LiBOB).

[0079] The concentration of the lithium salt may be in the range of about 0.1 M to about 2.0 M. If (e.g., when) the concentration of the lithium salt is within the described range, the electrolyte may have suitable or appropriate ion conductivity and viscosity, and thus may achieve excellent or appropriate performance, e.g., lithium ions may be efficiently moved.

[0080] Rechargeable lithium battery

[0081] In some embodiments, a rechargeable lithium battery may include a positive electrode; a negative electrode; and an electrolyte as described herein.

[0082] A rechargeable lithium battery of some embodiments includes an electrolyte, and thus may improve cycle-life characteristics and suppress or reduce an increase in resistance at room temperature and / or high temperature.

[0083] Positive electrode active material

[0084] The positive electrode may include a positive electrode active material.

[0085] The positive electrode active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions. For example, a composite oxide of one or more types (species) of lithium and a metal selected from cobalt, manganese, nickel and / or a combination thereof (e.g., any appropriate combination) may be used.

[0086] The composite oxide may be a lithium transition metal composite oxide, and specific examples may include lithium nickel-based oxides, lithium cobalt-based oxides, lithium manganese-based oxides, lithium iron phosphate-based compounds, cobalt-free lithium nickel manganese-based oxides and / or combinations thereof (e.g., any appropriate combination).

[0087] For example, a compound represented by any of the following chemical formulas may be used as the composite oxide: Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b- c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NeG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3(0≤f≤2); and Li a FePO4(0.90≤a≤1.8)

[0088] In the described chemical formula, A may be Ni, Co, Mn, and / or a combination thereof (e.g., any suitable combination); X may be Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, and / or a combination thereof (e.g., any suitable combination); D may be O, F, S, P, and / or a combination thereof (e.g., any suitable combination); G may be Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, and / or a combination thereof (e.g., any suitable combination); and L 1 It may be Mn, Al, and / or combinations thereof (eg, any suitable combination).

[0089] More specifically, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula 11.

[0090] Chemical formula 11

[0091] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1

[0092] In Chemical Formula 11, 0.9≤a1≤1.2, 0.6≤x1≤1, 0≤y1≤0.3, 0≤z1≤0.3, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1; M 1 and M 2 Each of them may be independently one or more elements selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W and Zr; and X may be one or more elements selected from F, P and S.

[0093] In Chemical Formula 11, 0.7≤x1≤1, 0≤y1≤0.2, and 0≤z1≤0.2; 0.75≤x1≤1, 0≤y1≤0.18, and 0≤z1≤0.18; 0.85≤x1≤1, 0≤y1≤0.15, and 0≤z1≤0.15; or 0.9≤x1≤1, 0≤y1≤0.1, and 0≤z1≤0.1.

[0094] For example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula 12. The lithium nickel-based composite oxide represented by Chemical Formula 12 may be a lithium nickel cobalt-based oxide.

[0095] Chemical formula 12

[0096] Li a2 Nix2 Co y2 M 3 z2 O 2-b2 X b2

[0097] In Chemical Formula 12, 0.9 ≤ a2 ≤ 1.8, 0.6 ≤ x2 < 1, 0 < y2 ≤ 0.3, 0 ≤ z2 ≤ 0.3, 0.9 ≤ x2 + y2 + z2 ≤ 1.1, and 0 ≤ b2 ≤ 0.1, M 3 may be one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from F, P, and S.

[0098] In Chemical Formula 12, 0.7 ≤ x2 < 1, 0 < y2 ≤ 0.2, and 0 ≤ z2 ≤ 0.2; 0.75 ≤ x2 ≤ 0.99, 0 < y2 ≤ 0.15, and 0 ≤ z2 ≤ 0.15; 0.85 ≤ x2 ≤ 0.99, 0.01 ≤ y2 ≤ 0.15, and 0.01 ≤ z2 ≤ 0.15; or 0.9 ≤ x2 ≤ 0.99, 0.01 ≤ y2 ≤ 0.1, and 0.01 ≤ z2 ≤ 0.1.

[0099] As an example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula 13. The lithium nickel-based composite oxide represented by Chemical Formula 13 may be a lithium nickel cobalt aluminum oxide or a lithium nickel cobalt manganese oxide.

[0100] Chemical Formula 13

[0101] Li a3 Ni x3 Co y3 M 4 z3 M 5 w3 O 2-b3 X b3

[0102] In Chemical Formula 13, 0.9 ≤ a3 ≤ 1.8, 0.6 ≤ x3 ≤ 0.98, 0.01 ≤ y3 ≤ 0.29, 0.01 ≤ z3 ≤ 0.29, 0 ≤ w3 ≤ 0.29, 0.9 ≤ x3 + y3 + z3 + w3 ≤ 1.1, and 0 ≤ b3 ≤ 0.1, M 4 may be one or more elements selected from Al and Mn, M 5 may be one or more elements selected from B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X may be one or more elements selected from F, P, and S.

[0103] In Chemical Formula 13, 0.7 ≤ x3 ≤ 0.98, 0.01 ≤ y3 ≤ 0.19, 0.01 ≤ z3 ≤ 0.19, and 0 ≤ w3 ≤ 0.19; 0.75 ≤ x3 ≤ 0.98, 0.01 ≤ y3 ≤ 0.16, 0.01 ≤ z3 ≤ 0.16, and 0 < w3 ≤ 0.16; 0.85 ≤ x3 ≤ 0.98, 0.01 ≤ y3 ≤ 0.14, 0.01 ≤ z3 ≤ 0.14, and 0 ≤ w3 ≤ 0.14; or 0.9 ≤ x3 ≤ 0.98, 0.01 ≤ y3 ≤ 0.09, 0.01 ≤ z3 ≤ 0.09, and 0 ≤ w3 ≤ 0.09.

[0104] As an example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula 14. The lithium nickel-based composite oxide represented by Chemical Formula 14 may be a cobalt-free lithium nickel manganese-based oxide.

[0105] Chemical Formula 14

[0106] Li a4 Ni x4 Mn y4 M 6 z4 O 2-b4 X b4

[0107] In Chemical Formula 14, 0.9 ≤ a4 ≤ 1.8, 0.6 ≤ x4 < 1, 0 < y4 ≤ 0.3, 0 ≤ z4 ≤ 0.3, 0.9 ≤ x4 + y4 + z4 ≤ 1.1, and 0 ≤ b4 ≤ 0.1, M 6 may be one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X may be one or more elements selected from F, P, and S.

[0108] In Chemical Formula 14, 0.7 ≤ x4 < 1, 0 < y4 ≤ 0.2, and 0 ≤ z4 ≤ 0.2; 0.75 ≤ x4 ≤ 0.99, 0 < y4 ≤ 0.15, and 0 ≤ z4 ≤ 0.15; 0.85 ≤ x4 ≤ 0.99, 0.01 ≤ y4 ≤ 0.15, and 0.01 ≤ z4 ≤ 0.15; or 0.9 ≤ x4 ≤ 0.99, 0.01 ≤ y4 ≤ 0.1, and 0.01 ≤ z4 ≤ 0.1.

[0109] If (for example, when) a transition metal dissolves out from the positive electrode active material during the operation of a rechargeable lithium battery and is reduced on the surface of the negative electrode, the structure of the surface of the negative electrode may be weakened. As a result, an increase in battery resistance and a reduction in cycle life may occur, and in the long run, lithium crystals may form, which may cause a short circuit between the positive electrode and the negative electrode.

[0110] On the contrary, recently, in order to cope with the cobalt consumption and cost increase, research on the so-called "cobalt-free positive electrode active material" is underway. The cobalt-free positive electrode active material refers to a positive electrode active material having a layered structure composed of nickel, manganese, etc. as main components and containing no cobalt in the positive electrode active material composition. In the rechargeable lithium battery of some embodiments, a type or kind of cobalt-free lithium nickel manganese-based oxide represented by Chemical Formula 14 can be used as the cobalt-free positive electrode active material.

[0111] However, due to the absence of cobalt, the positive electrode active material without cobalt has high structural instability, so there is a high possibility that nickel and / or manganese will be dissolved during the operation of the rechargeable lithium battery. In addition, this problem may become more serious at high temperatures.

[0112] Nevertheless, if (for example, when) an electrolyte prepared by adding a compound having a structure of two acid anhydrides connected by an aliphatic ring or an aromatic ring (Chemical Formula 1) is used, even if a positive electrode active material having a layered structure and not containing cobalt is used, a stable SEI film can improve cycle life characteristics and protect the negative electrode surface, and suppress or reduce the increase in resistance of the rechargeable lithium battery during operation at room temperature and / or high temperature.

[0113] Positive electrode

[0114] The positive electrode for a rechargeable lithium battery may include a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector. The positive electrode active material layer may include a positive electrode active material and may further include a binder and / or a conductive material.

[0115] The content (eg, amount) of the positive electrode active material may be about 90 wt % to about 99.5 wt % based on 100 wt % of the positive electrode active material layer.

[0116] In some embodiments, the positive electrode active material layer may further include a binder and a conductive material. At this time, the content (eg, amount) of the binder and the conductive material may be about 0.5 wt % to about 5 wt % based on 100 wt % of the positive electrode active material layer.

[0117] The binder is used to attach the positive electrode active material particles to each other well, and also to attach the positive electrode active material to the positive electrode current collector well. Examples of binders may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers including ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth) acrylated styrene-butadiene rubber, epoxy resin, (meth) acrylic resin, polyester resin, nylon, etc., as non-limiting examples.

[0118] Conductive materials can be used to impart conductivity (e.g., electrical conductivity) to the electrodes. Any material that does not cause chemical changes (e.g., does not cause undesirable chemical changes in a rechargeable lithium battery) and conducts electrons can be used in the battery. Examples of conductive materials may include carbon-based materials (such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes); metal-based materials containing copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fiber; conductive polymers (such as polyphenylene derivatives); or mixtures thereof.

[0119] Al foil may be used as a positive electrode current collector, but the present disclosure is not limited thereto.

[0120] Negative electrode active material

[0121] The negative electrode may include a negative electrode active material.

[0122] The negative electrode active material may be a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / dedoping lithium, or a transition metal oxide.

[0123] The material that reversibly intercalates / deintercalates lithium ions may include a carbon-based negative electrode active material, such as crystalline carbon, amorphous carbon, and / or a combination thereof (e.g., any suitable combination). The crystalline carbon may be graphite (such as amorphous, flaky, sheet-like, spherical or fibrous natural graphite or artificial graphite). The amorphous carbon may be soft carbon, hard carbon, a mesophase pitch carbonization product, calcined coke, etc.

[0124] The lithium metal alloy may include lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.

[0125] The material capable of being doped / undoped with lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may include silicon, a silicon-carbon composite (Si-C composite), SiO x(0 < x ≤ 2), Si-Q alloys (where Q is selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements (excluding Si), Group 15 elements, Group 16 elements, transition metals, rare earth elements, and / or combinations thereof (e.g., any suitable combination), such as Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and / or combinations thereof (e.g., any suitable combination)). The Sn-based negative electrode active material may include Sn, SnO2, SnO x (0 < x < 2), Sn-based alloys, and / or combinations thereof (e.g., any suitable combination).

[0126] The silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle size (D 50 ) may be, for example, about 0.5 micrometers (μm) to about 20 μm. According to some embodiments, the silicon-carbon composite may be in (or provided as) the form of silicon particles and amorphous carbon coated on the surface of the silicon particles. For example, the silicon-carbon composite may include secondary particles (cores) in which primary silicon particles are assembled and an amorphous carbon coating (shell) on the surface of the secondary particles. The amorphous carbon may also be between the primary silicon particles, and, for example, the primary silicon particles may be coated with amorphous carbon. The secondary particles may be dispersed in the amorphous carbon matrix (present).

[0127] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core containing crystalline carbon and silicon particles and amorphous carbon coated on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, and / or combinations thereof (e.g., any suitable combination). The amorphous carbon may include soft carbon or hard carbon, mesophase pitch carbonized products (e.g., coal pitch), and calcined coke.

[0128] If (e.g., when) the silicon-carbon composite includes silicon and amorphous carbon, based on 100 wt% of the silicon-carbon composite, the content (e.g., amount) of silicon may be 10 wt% to 50 wt%, and the content (e.g., amount) of amorphous carbon may be 50 wt% to 90 wt%. In one or more embodiments, if (e.g., when) the silicon-carbon composite includes silicon, amorphous carbon, and crystalline carbon, based on 100 wt% of the silicon-carbon composite, the content (e.g., amount) of silicon may be 10 wt% to 50 wt%, and the content (e.g., amount) of crystalline carbon may be 10 wt% to 70 wt%, and the content (e.g., amount) of amorphous carbon may be 20 wt% to 40 wt%.

[0129] Additionally, the thickness of the amorphous carbon coating can be from about 5 nanometers (nm) to about 100 nm. The average particle diameter (D 50 ) of the silicon particles (primary particles) can be from about 10 nm to about 1 μm or from about 10 nm to about 200 nm. The silicon particles can exist as elemental silicon, in the form of (or provided as) a silicon alloy, or in an oxidized form of silicon. The oxidized form of silicon (or provided as) can be represented by SiO x (0 < x ≤ 2). In some embodiments, the atomic content (e.g., amount) ratio of Si:O indicating the degree of oxidation can be from 99:1 to 33:67. In this specification, as used herein, if (e.g., when) no other definition is provided otherwise, the average particle diameter (D 50 ) indicates the diameter of the particles with a cumulative volume of about 50 volume % in the particle size distribution.

[0130] Si-based negative electrode active materials or Sn-based negative electrode active materials can be used in combination with carbon-based negative electrode active materials. If (e.g., when) a mixture of Si-based negative electrode active materials or Sn-based negative electrode active materials and carbon-based negative electrode active materials is used, the mixing ratio can be from about 1:99 to about 90:10 by weight.

[0131] Negative electrode

[0132] The negative electrode for a rechargeable lithium battery includes a negative electrode current collector and a negative electrode active material layer on the negative electrode current collector. The negative electrode active material layer includes negative electrode active materials and can further include a binder and / or a conductive material.

[0133] Based on 100 wt% of the negative electrode active material layer, the content (e.g., amount) of the negative electrode active material can be from about 95 wt% to about 99.5 wt%. Based on 100 wt% of the negative electrode active material layer, the content (e.g., amount) of the binder can be from about 0.5 wt% to about 5 wt%. Based on 100 wt% of the negative electrode active material layer, the content (e.g., amount) of the conductive material can be from about 0.5 wt% to about 5 wt%. For example, the negative electrode active material layer can include from about 90 wt% to about 99 wt% of the negative electrode active material, from about 0.5 wt% to about 5 wt% of the binder, and from about 0.5 wt% to about 5 wt% of the conductive material.

[0134] The binder can be used to attach the negative electrode active material particles to each other well and also attach the negative electrode active material well to the negative electrode current collector. The binder can include a non-aqueous binder, an aqueous binder, a dry binder, and / or a combination thereof (e.g., any suitable combination).

[0135] The non-aqueous binder may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, and / or combinations thereof (eg, any suitable combination).

[0136] The aqueous binder can be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol and / or combinations thereof (e.g., any suitable combination).

[0137] If (for example, when) an aqueous binder is used as a negative electrode binder, it may further include a cellulose compound capable of imparting viscosity. The cellulose compound includes one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, and alkali metal salts thereof. The alkali metal may be Na, K, and / or Li.

[0138] The dry binder may be a polymer material capable of fiberization, and may be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, and / or combinations thereof (eg, any appropriate combination).

[0139] A conductive material is included to provide electrode conductivity, and any conductive material can be used as the conductive material unless it causes a chemical change. Examples of the conductive material may be a carbon-based material (such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube, etc.); a metal-based material containing copper, nickel, aluminum, silver, etc. in the form of a metal powder or metal fiber (or providing a metal powder or metal fiber); a conductive polymer (such as a polyphenylene derivative); or a mixture thereof.

[0140] The negative electrode current collector may include one selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof (eg, any appropriate combination), but the present disclosure is not limited thereto.

[0141] Diaphragm

[0142] Depending on the type or kind of rechargeable lithium battery, the separator may be present between the positive electrode and the negative electrode. The separator may include a polyethylene separator, a polypropylene separator, a polyvinylidene fluoride separator, or a multilayer film of two or more layers thereof (such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, a polypropylene / polyethylene / polypropylene three-layer separator, etc.).

[0143] The separator may include a porous substrate and a coating on one or both (eg, simultaneously) surfaces (eg, opposite surfaces) of the porous substrate, the coating including an organic material, an inorganic material, and / or (eg, any suitable) combination thereof.

[0144] The porous substrate may be a polymer film formed from any one selected from the following: polyolefins (such as polyethylene and polypropylene), polyesters (such as polyethylene terephthalate and polybutylene terephthalate), polyacetals, polyamides, polyimides, polycarbonates, polyetherketones, polyaryletherketones, polyetherimides, polyamideimides, polybenzimidazoles, polyethersulfones, polyphenylene oxides, cyclic olefin copolymers, polyphenylene sulfide, polyethylene naphthalate, glass fibers, Teflon and polytetrafluoroethylene, or copolymers or mixtures of two or more thereof.

[0145] The porous substrate may have a thickness of about 1 μm to about 40 μm (eg, about 1 μm to about 30 μm, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 10 μm to about 15 μm).

[0146] The organic material may include a (meth)acryl-based copolymer including a first structural unit derived from (meth)acrylamide and a second structural unit including at least one of a structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamide sulfonic acid or a salt thereof.

[0147] The inorganic material may include inorganic particles selected from Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, SrTiO3, BaTiO3, Mg(OH)2, boehmite, and / or combinations thereof (e.g., any suitable combination), but the present disclosure is not limited thereto. The average particle size (D 50 ) may be from about 1 nm to about 2000 nm (eg, from about 100 nm to about 1000 nm or from about 100 nm to about 700 nm).

[0148] An organic material and an inorganic material may be mixed in one coating layer, or a coating layer including an organic material and a coating layer including an inorganic material may be stacked.

[0149] The coating layer may have a thickness of about 0.5 μm to about 20 μm (eg, about 1 μm to about 10 μm or about 1 μm to about 5 μm).

[0150] Rechargeable lithium battery

[0151] The rechargeable lithium batteries may be classified into cylindrical or cylindrical-type batteries, prismatic or prismatic-type batteries, pouch or pouch-type batteries, or coin or coin-type batteries, etc., depending on their shapes. Figure 1 to Figure 3 Schematic diagram showing a rechargeable lithium battery according to some embodiments. Figure 1 to Figure 3 , the rechargeable lithium battery 100 includes an electrode assembly 40 and a case 50 accommodating the electrode assembly 40, the electrode assembly 40 having a separator 30 interposed between a positive electrode 10 and a negative electrode 20. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte. Figure 1 As shown, the rechargeable lithium battery 100 may include a sealing member 60 that seals the housing 50, and as shown in FIG. Figure 3 As shown, it may further include an electrode tab 70 serving as an electric path for guiding current generated in the electrode assembly 40 to the outside.

[0152] Terms such as "substantially," "about," and "approximately" are used as relative terms rather than terms of degree, and are intended to account for the inherent deviations in measured or calculated values ​​that would be recognized by one of ordinary skill in the art. They may include the stated value and an acceptable range of deviation determined by one of ordinary skill in the art taking into account the limitations and errors associated with the measurement of that quantity. For example, "about" may refer to one or more standard deviations, or ±30%, 20%, 10%, or 5% of the stated value.

[0153] The numerical ranges disclosed herein include and are intended to disclose all sub-ranges of the same numerical precision. For example, the range of "1.0 to 10.0" includes all sub-ranges with a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as, for example, 2.4 to 7.6. Therefore, the applicant reserves the right to amend this specification (including the claims) to explicitly set forth any sub-ranges contained within the range explicitly set forth herein.

[0154] Here, a process listed in a particular order should not necessarily mean that the invention or claims require that particular order. That is, the general rule is that unless the steps, tasks or actions of a process (e.g., method) actually set out an order, these steps, tasks or actions should not be interpreted as requiring an order.

[0155] Hereinafter, embodiments of the present disclosure and comparative examples will be described. The following examples are merely examples of the present disclosure, and the present disclosure is not limited to the following examples.

[0156] Example

[0157] Electrolyte and rechargeable lithium battery cell manufacturing

[0158] Example 1

[0159] (1) Preparation of electrolyte

[0160] The electrolyte was prepared by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 2:4:4, dissolving 1.5M LiPF6 in a non-aqueous organic solvent, and adding 0.05wt% of the additive represented by Chemical Formula 1-1 (product name: SKU 412287-100G, manufacturer: Sigma-Aldrich).

[0161] Chemical formula 1-1

[0162]

[0163] In the composition of the electrolyte, the content (eg, amount) of the additive, "wt %" is based on 100 wt % of the total electrolyte (lithium salt+nonaqueous organic solvent+additive).

[0164] (2) Manufacturing of rechargeable lithium battery cells

[0165] LiNi as the positive electrode active material 0.75 Mn 0.23 Al 0.02 O2, polyvinylidene fluoride as a binder, and acetylene black as a conductive material were mixed at a weight ratio of 96:3:1, respectively, and then dispersed in N-methylpyrrolidone to prepare a positive electrode active material slurry.

[0166] The positive electrode active material slurry was coated on a 15 micrometer (μm) thick Al foil, dried at 100° C., and pressed to manufacture a positive electrode.

[0167] A mixture of artificial graphite and Si—C composite at a weight ratio of 93:7 was used as a negative electrode active material, and the negative electrode active material, styrene-butadiene rubber binder, and carboxymethyl cellulose were dispersed in distilled water at a weight ratio of 98:1:1 to prepare a negative electrode active material slurry.

[0168] The Si-C composite includes a core including artificial graphite and silicon particles, and coal tar pitch coated on the surface of the core.

[0169] The negative electrode active material slurry was coated on a 10 μm thick Cu foil, dried at 100° C., and pressed to produce a negative electrode.

[0170] An electrode assembly was manufactured by assembling a positive electrode, a negative electrode, and a separator made of polyethylene having a thickness of 10 μm, and an electrolyte was injected to manufacture a rechargeable lithium battery cell.

[0171] Example 2

[0172] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-1 was added in an amount of 0.1 wt %.

[0173] Example 3

[0174] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-1 was added in an amount of 0.5 wt %.

[0175] Example 4

[0176] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-1 was added in an amount of 1.0 wt %.

[0177] Example 5

[0178] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-1 was added in an amount of 3.0 wt %.

[0179] Example 6

[0180] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-2 (product name: C2419-25G, manufacturer: TCI Chemical Industry) was added in an amount of 0.05 wt % instead of the additive represented by Chemical Formula 1-1.

[0181] Chemical formula 1-2

[0182]

[0183] Example 7

[0184] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-2 was added in an amount of 0.1 wt % instead of the additive represented by Chemical Formula 1-1.

[0185] Example 8

[0186] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-2 was added in an amount of 0.5 wt % instead of the additive represented by Chemical Formula 1-1.

[0187] Example 9

[0188] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-2 was added in an amount of 1.0 wt % instead of the additive represented by Chemical Formula 1-1.

[0189] Example 10

[0190] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula 1-2 was added in an amount of 3.0 wt % instead of the additive represented by Chemical Formula 1-1.

[0191] Embodiment 11

[0192] The electrolyte and the rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that LiNi 0.9 Co 0.05 Al 0.05 O2 replaces LiNi 0.75 Mn 0.23 Al 0.02 O2 is used as the positive electrode active material.

[0193] Comparative Example 1 (reference)

[0194] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that no additive was added (eg, no additive was added at all).

[0195] Comparative Example 2

[0196] An electrolyte and a rechargeable lithium battery cell were manufactured in substantially the same manner as Example 1, except that the additive represented by Chemical Formula A was added in an amount of 0.5 wt % instead of the additive represented by Chemical Formula 1-1.

[0197] Chemical formula A

[0198]

[0199] Evaluation Example

[0200] Rechargeable lithium battery cells manufactured by using the electrolytes according to Examples 1 to 11 and Comparative Examples 1 and 2, respectively, were evaluated as follows, and the results are shown in Tables 1 to 2.

[0201] Evaluation 1: Evaluation of room temperature charge / discharge cycle life characteristics

[0202] The rechargeable lithium battery cells according to Examples 1 to 11 and Comparative Examples 1 and 2 were charged and discharged under the following conditions to evaluate cycle-life characteristics, and the results are shown in Table 1.

[0203] The rechargeable lithium battery cells were charged and discharged for 800 cycles under the conditions of 0.33C charge (CC / CV, 4.45V, 0.025C cutoff) / 1.0C discharge (CC, 2.5V cutoff) at 25°C to measure the capacity retention rate and direct current internal resistance (DC-IR) change rate.

[0204] The capacity retention rate was calculated according to Equation 1, and the DC-IR change rate was calculated according to Equation 2 based on the voltage change while discharging for 30 seconds by applying a current of SOC 50C (a current equivalent to 50% of the charge capacity based on 100% of the overall charge capacity of the rechargeable lithium battery cell).

[0205] Equation 1

[0206] Capacity retention rate = (discharge capacity after 800th cycle / discharge capacity after 1st cycle)*100

[0207] Equation 2

[0208] DC-IR change rate = {(DC-IR after the 800th cycle) / (DC-IR after the 1st cycle)}*100

[0209] Table 1

[0210]

[0211] Referring to Table 1, if (eg, when) the additive according to some embodiments is used at room temperature, not only the cycle-life characteristics are improved but also the resistance increase is suppressed or reduced.

[0212] Evaluation 2: Evaluation of high temperature storage characteristics

[0213] Capacity retention rate / capacity recovery rate / DC-IR change rate

[0214] (1) Capacity retention rate and capacity recovery rate

[0215] Each of the rechargeable lithium battery cells according to Examples 1 to 11 and Comparative Examples 1 and 2 was charged and discharged once at 0.33 C to measure the charge and discharge capacity (before high-temperature storage).

[0216] In one or more embodiments, each of the rechargeable lithium battery cells of Examples 1 to 11 and Comparative Examples 1 and 2 is charged to SOC 100% (a state of charging to 100% of the charge capacity based on 100% of the overall charge capacity of the rechargeable lithium battery cell), stored at 60° C. for 60 days, and then discharged to 3.0 V at 0.33 C under constant current conditions to measure the initial discharge capacity.

[0217] The rechargeable lithium battery cell was recharged to 4.3V at a constant current of 0.33C, cut off at a termination current of 0.02C, and discharged to 3.0V at a constant current of 0.33C to measure the discharge capacity twice. The ratio of the first discharge capacity to the initial discharge capacity was calculated as the capacity retention rate (retention capacity), and the ratio of the second discharge capacity to the initial discharge capacity was calculated as the capacity recovery rate (recovery capacity).

[0218] (2) DC-IR change rate

[0219] The initial DC-IR of each of the rechargeable lithium battery cells according to Examples 1 to 11 and Comparative Examples 1 and 2 was measured using ΔV / ΔI (voltage change / current change), and the rechargeable lithium battery cells were charged to a full charge state (SOC 100%) as the internal maximum energy state, and the DC-IR was measured after being stored at a high temperature of 60°C for 60 days to calculate the DC-IR change rate (%), and the results are shown in Table 2.

[0220] Equation 3

[0221] DC-IR change rate = (DC-IR after 60 days / initial DC-IR)*100

[0222] Table 2

[0223]

[0224] Referring to Table 2, compared with the rechargeable lithium battery cells of Comparative Examples 1 and 2, the rechargeable lithium battery cells of Examples 1 to 11 each exhibited not only improved capacity retention and improved capacity recovery during high temperature storage, but also each had resistance increase suppressed or reduced.

[0225] Summarize

[0226] Referring to Tables 1 and 2, compared with Comparative Example 1 in which no additive is used, Examples 1 to 11 each using a compound having a structure in which two acid anhydrides are connected by an aliphatic ring or an aromatic ring (Chemical Formula 1) as an additive show improved high temperature storage characteristics and room temperature charge and discharge characteristics of a rechargeable lithium battery cell. For example, Examples 1 to 10 each using a positive electrode active material that does not contain cobalt show significant effects.

[0227] In contrast, in Comparative Example 1 in which no additive is used and Comparative Example 2 in which a linear acid anhydride compound is used as an additive, the additive is reduced and decomposed on the negative electrode surface and forms an unstable film, and the cycle life of the rechargeable lithium battery cell is deteriorated and the resistance is increased. This phenomenon becomes more obvious (e.g., noticeable) if (e.g., when) stored at high temperature.

[0228] According to the battery management system (BMS) device and / or any other related device or component of the embodiments of the present invention described herein, any appropriate hardware, firmware (e.g., a dedicated integrated circuit), software, or a combination of software, firmware, and hardware may be used for implementation. For example, the various components of the device may be formed on an integrated circuit (IC) chip or on separate IC chips. Further, the various components of the device may be implemented on a flexible printed circuit film, a tape carrier package (TCP), or a printed circuit board (PCB), or formed on a substrate. Further, the various components of the device may be processes or threads running on one or more processors in one or more computing devices, which execute computer program instructions and interact with other system components to perform the various functions described herein. The computer program instructions are stored in a memory, which may be implemented in a computing device using a standard memory device, such as, for example, a random access memory (RAM). The computer program instructions may also be stored in other non-transitory computer-readable media, such as, for example, a CD-ROM or a flash drive, etc. Moreover, those skilled in the art will recognize that, without departing from the scope of the embodiments of the present disclosure, the functions of various computing devices may be combined or integrated into a single computing device, or the functions of a particular computing device may be distributed on one or more other computing devices.

[0229] Although the present disclosure has been described in conjunction with exemplary embodiments currently considered to be practical, it should be understood that the present disclosure is not limited to the disclosed embodiments. However, on the contrary, the present disclosure is intended to cover one or more suitable modifications and equivalents included within the spirit and scope of the appended claims and their equivalents.

Claims

1. An additive, the additive is represented by chemical formula 1: Chemical formula 1 In Chemical Formula 1, A is a substituted or unsubstituted C3-C10 aliphatic ring or a substituted or unsubstituted C6-C20 aromatic ring; and X 1 and X 2 are each independently O or S, The additive is used in electrolytes for rechargeable lithium batteries.

2. The additive according to claim 1, wherein A is a cyclohexane ring or a benzene ring.

3. The additive according to claim 1, wherein X 1 and X 2 Each is O.

4. The additive according to claim 1, wherein The additive is represented by Chemical Formula 1-1 or Chemical Formula 1-2: Chemical formula 1-1 Chemical formula 1-2 5. An electrolyte comprising: Non-aqueous organic solvents; Lithium salts; and The additive according to any one of claims 1 to 4, The electrolyte is used in rechargeable lithium batteries.

6. The electrolyte according to claim 5, wherein The electrolyte includes the additive in an amount of 0.05 wt % to 3.0 wt % based on 100 wt % of the electrolyte.

7. The electrolyte according to claim 5, wherein The electrolyte includes the additive in an amount of 0.5 wt % to 3.0 wt % based on 100 wt % of the electrolyte.

8. The electrolyte according to claim 5, wherein The non-aqueous organic solvent includes at least one selected from carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents and aprotic solvents.

9. The electrolyte according to claim 5, wherein The non-aqueous organic solvent includes ethylene carbonate, ethylmethyl carbonate and dimethyl carbonate.

10. The electrolyte of claim 9, wherein The volume ratio of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate is 2:4:

4.

11. A rechargeable lithium battery, comprising: Positive electrode; Negative electrode; and The electrolyte according to any one of claims 5 to 10.

12. The rechargeable lithium battery of claim 11, wherein The positive electrode includes a positive electrode active material including a lithium nickel-based composite oxide.

13. The rechargeable lithium battery of claim 12, wherein The lithium nickel composite oxide is represented by Chemical Formula 11: Chemical formula 11 Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 In Chemical Formula 11, 0.9≤a1≤1.2, 0.6≤x1≤1, 0≤y1≤0.3, 0≤z1≤0.3, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1; M 1 and M 2 Each is independently at least one element selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W and Zr; and X is at least one element selected from F, P and S.

14. The rechargeable lithium battery of claim 11, wherein The rechargeable lithium battery includes a separator between the positive electrode and the negative electrode.

15. A method for manufacturing a rechargeable lithium battery, the method comprising: preparing an electrolyte comprising a non-aqueous organic solvent, a lithium salt and an additive as claimed in any one of claims 5 to 10; preparing a positive electrode; preparing a negative electrode; preparing an electrode assembly including the positive electrode, the negative electrode and a separator; as well as The electrolyte is injected into the electrode assembly.