Electrolyte and lithium ion battery
By using electrolyte of bicyclic etherketone compound A in lithium-ion batteries, the performance degradation of lithium-ion batteries in fast charging and high-nickel positive electrode materials applications is solved, and the performance improvement of high- and low-temperature performance and fast charging capabilities are achieved. Extends the battery cycle life.
Patent Information
- Application Number
- CN202411143815.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-20
AI Technical Summary
Existing lithium-ion batteries are prone to lithium-ion deposition, electrolyte oxidation and interface side reactions in fast charging and high-nickel ternary cathode materials applications, resulting in reduced performance and difficult to meet high capacity and fast charging requirements.
Using an electrolyte containing bicyclic etherketone compound A, which has low oxidation potential and low viscosity, forms a thin interface layer to reduce the ion transport path, stabilize the lithium ion transport channel, and complex through a dual oxygen-containing heterocyclic structure. The residual alkali on the surface of high-nickel positive electrode material inhibits interfacial side reactions.
Improves the high-temperature and low-temperature performance of lithium-ion batteries, supports fast charging characteristics, extends the battery's cycle life and improves high-temperature storage performance.
Smart Images

Figure CN119092828A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to an electrolyte and a lithium ion battery. Background Art
[0002] As a green and environmentally friendly high-energy battery, secondary batteries are currently the most ideal and most promising rechargeable batteries in the world. In particular, lithium-ion batteries among secondary batteries have a series of advantages over other batteries, such as no memory effect, fast charging and discharging, high energy density, long cycle life and no environmental pollution. Therefore, they are widely used in small electronic devices such as laptops, cameras, mobile phones, electronic watches, etc., as well as large power transmission equipment such as electric vehicles and energy storage. Today, with the increasing requirements for lithium-ion battery capacity in pure electric vehicles, hybrid vehicles and portable energy storage devices, people are looking forward to the development of lithium-ion batteries with fast charging capabilities and high capacity to improve the convenience of people's lives.
[0003] At present, the industry increases the charging speed of lithium-ion batteries by increasing the charging current. However, the increase in charging speed leads to local lithium deposition. At the same time, since the rate of lithium ion embedding into graphite is lower than the rate of lithium ion migration, a large amount of lithium is accumulated, which will further aggravate the deposition of lithium ions and make lithium dendrites more likely to form. Lithium dendrites will cause the electrode electrolyte interface to continuously decompose and regenerate, and the electrolyte will continue to be consumed, eventually leading to poor performance of lithium-ion batteries.
[0004] In addition, one of the effective ways to increase the capacity of power batteries is to increase the nickel content in ternary cathode materials. This is the trend of battery development and an inevitable requirement for the development of new energy vehicles. Although at the same cut-off voltage, the higher the nickel content of the ternary cathode material, the more Li + , thus achieving higher capacity output; however, a large amount of Li + The structure of the high-lithium ion cathode material after release is very unstable, which leads to the problem of material cycle capacity decay and decreased thermal stability. In addition, the surface residual alkali content of high-nickel ternary cathode materials is relatively high. Conventional electrolytes are easily oxidized and decomposed on the cathode surface in high-nickel batteries, especially under fast charging conditions, which will accelerate the oxidation and decomposition of the electrolyte and cause the cathode material to deteriorate.
[0005] Therefore, how to provide a lithium-ion battery with good comprehensive performance is a technical problem that needs to be solved urgently. Summary of the invention
[0006] The object of the present invention is to provide an electrolyte and a lithium ion battery, wherein the electrolyte has better high-temperature and low-temperature performance, is conducive to the rapid migration of ions under the condition of fast charging of the battery, and meets the requirements of high capacity and fast charging of secondary batteries.
[0007] In order to achieve the above object, the present invention provides an electrolyte, comprising an electrolyte salt, an organic solvent and an additive, wherein the additive comprises a compound A as shown in structural formula I. wherein R1 to R4 are each independently C=R5 or CR6R7, R5 is an alkylene group, and R6 to R7 are each independently hydrogen, halogen, C1 to C6 alkyl, C2 to C6 alkenyl, C2 to C6 alkynyl or cyano. The viscosity of compound A is 1 to 3 mba / cm.
[0008]
[0009] Compared with the prior art, the electrolyte of the present invention contains compound A, which is a bicyclic ether ketone compound, so it has a relatively low oxidation potential and viscosity (viscosity is 1 to 3 mba / cm). Its low potential characteristic can be oxidized before the solvent to form a thinner interface layer on the electrode surface, which can reduce the ion transmission path and improve the gas production problem of the battery under high voltage. In addition, the interface layer is not easy to shrink at low temperatures, and can maintain the lithium ion transmission channel at low temperatures to improve the low temperature (such as -20°C) performance of lithium-ion batteries. The low viscosity characteristic is also conducive to the rapid migration of ions under fast charging conditions, and can support the fast charging characteristics of secondary batteries. Furthermore, compound A is a dioxygen-containing heterocyclic structure, which can complex the residual alkali on the surface of the high-nickel ternary positive electrode material to reduce the interfacial side reactions of the battery during the cycle and storage process, effectively inhibit the decomposition of the SEI film interface, and thus improve the high temperature storage and high temperature cycle performance of the secondary battery.
[0010] Among them, the alkylene group may be methylene, ethylene, propylene, etc. The halogen may be fluorine or chlorine. The C1-C6 alkyl group represents an alkyl group with 1 to 6 carbon atoms, which may be a chain alkyl group or a cycloalkyl group, and may be, but not limited to, methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, pentyl, and cyclohexyl, etc. The C2-C6 alkenyl group represents an alkenyl group with 2 to 6 carbon atoms, which may be a chain alkenyl group or a cycloalkenyl group, and may be, but not limited to, vinyl, propenyl, isopropenyl, butenyl, sec-butenyl, tert-butenyl, pentenyl, and cyclohexenyl, etc. The C2-C6 alkynyl group represents an alkynyl group with 2 to 6 carbon atoms, which may be a chain alkynyl group or a cycloalkynyl group, and may be, but not limited to, ethynyl, propynyl, isopropynyl, butynyl, sec-butynyl, tert-butynyl, pentynyl, and cyclohexynyl, etc. The cyano group refers to a group containing -CN. Preferably, R1 to R4 are each independently C=CH2 or CR6R7, and R6 to R7 are each independently hydrogen, C1 to C3 alkyl, C2 to C3 alkenyl, or C2 to C3 alkynyl.
[0011] As a technical solution of the present invention, compound A is at least one selected from compounds 1 to 6.
[0012]
[0013] As a technical solution of the present invention, the mass of compound A accounts for 0.1% to 5.0% of the total mass of the electrolyte. As an example, the mass of compound A accounts for 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0% of the total mass of the electrolyte, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0014] As a technical solution of the present invention, the electrolyte salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethylsulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium methanesulfonate (LiCH3SO3), lithium trifluoromethylsulfonate (LiCF3SO3), lithium fluorosulfonate (LiSO2F), lithium bis(oxalate)borate (LiBC4O8), lithium difluorooxalate borate (LiBF2C2O4), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalate)phosphate (LiDFBP), lithium diphosphate (LiPO2F2), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and lower aliphatic lithium carboxylates. Further, lower aliphatic lithium carboxylates include but are not limited to lithium chloroborane, lithium tetraphenylborate, lithium imide salts, etc.
[0015] As a technical solution of the present invention, the mass of the electrolyte salt accounts for 5-25% of the total mass of the electrolyte. Further, the mass of the electrolyte salt accounts for 6-20% of the total mass of the electrolyte, and preferably, the mass of the electrolyte salt accounts for 8-18% of the total mass of the electrolyte. As an example, the mass of the electrolyte salt accounts for 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 24% of the total mass of the electrolyte, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0016] As a technical solution of the present invention, the organic solvent includes at least one of carbonate, carboxylate and ether compounds. Further, carbonate includes but is not limited to cyclic carbonate and chain carbonate. Cyclic carbonate may be but is not limited to ethylene carbonate (EC), propylene carbonate, butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC) or their derivatives. Chain carbonate includes but is not limited to dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC). Carboxylate includes but is not limited to cyclic carboxylate and chain carboxylate. Cyclic carboxylate specifically may include but is not limited to at least one of γ-butyrolactone, γ-valerolactone and δ-valerolactone. Chain carboxylate includes but is not limited to at least one of methyl acetate (MA), ethyl acetate (EA), propyl acetate (EP), butyl acetate, propyl propionate (PP) and butyl propionate. Ether compounds include cyclic ethers or chain ethers. Cyclic ethers include, but are not limited to, at least one of 1,3-dioxolane (DOL), 1,4-dioxolane (DX), crown ethers, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH3-THF) and 2-trifluoromethyltetrahydrofuran (2-CF3-THF). Chain ethers include, but are not limited to, at least one of dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether and diethylene glycol dimethyl ether.
[0017] As a technical solution of the present invention, the electrolyte also includes an auxiliary agent, which is selected from vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate, succinic anhydride, maleic anhydride, 2-methylmaleic anhydride, methyl carbonate-2-propynyl ester, tetravinylsilane, triallyl isocyanurate, hexamethylene diisocyanate, o-phenanthroline, terephthalate At least one of isocyanate, 2,4-toluene diisocyanate, N-phenyl bis(trifluoromethanesulfonyl)imide, vinyl bissulfate, phenyl methanesulfonate, vinyl bissulfate, bis-spiro propylene sulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, methacrylate isocyanatoethyl, methanedisulfonic acid methylene ester, tri(trimethylsilyl)borate, tri(trimethylsilyl)phosphate and tri(vinyldimethylsilyl)phosphate. As an example, the auxiliary agent is fluoroethylene carbonate (FEC), and the auxiliary agent is a mixture of vinylene carbonate and fluoroethylene carbonate.
[0018] As a technical solution of the present invention, the mass of the additive accounts for 0.1-5.0% of the total mass of the electrolyte. Further, the mass of the additive accounts for 0.2-2.0% of the total mass of the electrolyte. By way of example, the mass of the additive accounts for 0.1%, 0.2%, 0.5%, 0.8%, 1.0%, 1.5%, 2.0%, 2.2%, 2.5%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, 4.2%, 4.5%, 4.8%, 5.0% of the total mass of the electrolyte, but is not limited to the listed values, and other unlisted values within this numerical range are equally applicable.
[0019] On the other hand, the present invention also provides a lithium-ion battery, including a positive electrode material, a negative electrode material, and the above-mentioned electrolyte. This lithium-ion battery not only has good high-temperature storage and high-temperature cycling performance, but also has good low-temperature performance, especially good low-temperature performance at -20°C.
[0020] As a technical solution of the present invention, the positive electrode material is LiNi x Co y Mn z M 1-x-y-z O2 or LiNi x Co y Al z M 1-x-y- z O2, where M is any one of Mg, Cu, Zn, Sn, B, Ga, Cr, Sr, V, and Ti, 0.5≤x<1.0, 0<y<1.0, 0<z<1.0, 0.9<x + y + z≤1.0. The negative electrode material includes at least one of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, and a lithium negative electrode. Among them, the carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, mesophase carbon microspheres, etc. The silicon-based negative electrode may include silicon materials, silicon oxides, silicon-carbon composite materials, and silicon alloy materials, etc. The tin-based negative electrode may include tin, tin-carbon, tin-oxygen, and tin metal compounds. The lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium-silicon alloy, a lithium-sodium alloy, a lithium-potassium alloy, a lithium-aluminum alloy, a lithium-tin alloy, and a lithium-indium alloy. Specific Embodiments
[0021] In order to further illustrate the purpose, technical solution, and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that for those not specifying specific conditions in the embodiments and comparative examples, they can be carried out according to conventional conditions or conditions recommended by the manufacturer. For reagents or instruments not indicating the manufacturer, they are all conventional products that can be obtained through commercial channels.
[0022] Example 1
[0023] 1.1 Preparation of the electrolyte:
[0024] In a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a mass ratio of 2:1:5:2 to obtain a mixed solvent as an organic solvent, and compound 1 was added to obtain a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4°C) for 2 hours and then taken out. In a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide were slowly added to the mixed solution, and the electrolyte was prepared after mixing evenly.
[0025] 1.2 Preparation of positive electrode:
[0026] The ternary material LiNi 0.8 Co 0.1 Mn 0.1 Zr 0.03 O2, conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 96.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector. The coating amount is 324g / m 2 , dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and after slitting, dried at 85°C for 4 hours under vacuum conditions, and the tabs were welded to make lithium-ion battery positive electrodes that meet the requirements.
[0027] 1.3 Preparation of negative electrode sheet:
[0028] Artificial graphite and silicon are mixed in a mass ratio of 90:10, and then mixed with conductive agent SuperP, thickener CMC, and adhesive SBR (styrene-butadiene rubber emulsion) in a mass ratio of 95:1.5:1.0:2.5 to make a slurry, mix evenly, apply the mixed slurry on both sides of the copper foil, dry and roll to obtain a negative electrode sheet, and make a lithium-ion battery negative electrode sheet that meets the requirements.
[0029] 1.4 Preparation of lithium-ion batteries:
[0030] The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are laminated to form a lithium-ion battery with a thickness of 4.7mm, a width of 55mm and a length of 60mm. The battery is vacuum-baked at 75°C for 10h and the above electrolyte is injected. After standing for 24h, the battery is charged to 4.45V with a constant current of 0.1C (180mA), and then charged at a constant voltage of 4.45V until the current drops to 0.05C (90mA); then discharged to 3.0V with 0.2C (180mA), and the charge and discharge are repeated twice. Finally, the battery is charged to 3.8V with 0.2C (180mA) to complete the production of the lithium-ion battery.
[0031] The components and contents of the electrolytes of Examples 1 to 19 and Comparative Examples 1 to 8 are shown in Table 1, wherein the preparation processes of the lithium ion battery electrolytes, positive electrode sheets, negative electrode sheets, and lithium ion batteries of Examples 1 to 19 and Comparative Examples 1 to 8 are the same as those of Example 1. The auxiliary agent is added together with the additive.
[0032] Table 1 Compositions of the electrolytes of the embodiments and comparative examples
[0033]
[0034]
[0035]
[0036] The lithium ion batteries prepared in Examples 1 to 19 and Comparative Examples 1 to 8 were subjected to high temperature storage performance test, high temperature cycle performance test, room temperature fast charge cycle performance test, and low temperature performance test under the following conditions. The results are shown in Table 2.
[0037] (1) High temperature storage performance test
[0038] At room temperature (25°C), the lithium-ion battery was charged and discharged at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.4V, and then the battery was charged to 4.4V under 0.5C constant current and constant voltage conditions, and the battery thickness was measured (the thickness was recorded as D0); the battery was placed in a 60°C oven for 30 days, taken out and the battery thickness was measured (the thickness was recorded as D1); the battery was placed in a 25°C environment and discharged at 0.5C (the discharge capacity was recorded as C1); the lithium-ion battery was continued to be charged and discharged at room temperature (25°C) at 0.5C / 0.5C (the battery discharge capacity was recorded as C2), with an upper limit voltage of 4.4V, and the capacity retention rate, capacity recovery rate and thickness expansion rate were calculated.
[0039] Capacity retention rate = (C1 / C0)*100%
[0040] Capacity recovery rate = (C2 / C0)*100%
[0041] Thickness expansion rate = (D1 / D0)*100%
[0042] (2) Normal temperature cycle performance test
[0043] At room temperature (25°C), the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 4.0C / 1.0C for 500 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0044] Capacity retention rate = (C1 / C0)*100%
[0045] (3) High temperature cycle test
[0046] Under high temperature (45°C) conditions, the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 1.0C / 1.0C for 400 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0047] Capacity retention rate = (C1 / C0)*100%
[0048] (4) Low temperature performance test
[0049] At room temperature (25°C), the lithium-ion battery is charged and discharged at 0.5C / 0.5 (battery cut-off voltage is 3.0V, discharge capacity is C0), and the upper limit voltage is 4.4V (cut-off current 0.05C). Then the battery is fully charged to 4.4V (cut-off current 0.05C) at 0.5C at room temperature (25°C), and then the battery is transferred to -20°C and left for 4h, and discharged to 3.0V at 0.5C, and the discharge capacity is C1. The capacity retention rate is calculated.
[0050] Capacity retention rate = (C1 / C0)*100%
[0051] Table 2 Test results of lithium-ion battery performance
[0052]
[0053]
[0054] From the results in Table 2, it can be seen that compared with Comparative Examples 1 to 8, the comprehensive performance of Examples 1 to 19 is better. This is because the electrolytes of Examples 1 to 19 contain compound A, which is a bicyclic ether ketone compound, so it has a relatively low oxidation potential and viscosity. Its low potential characteristic can be oxidized before the solvent to form a thinner interface layer on the electrode surface, which can reduce the ion transmission path and improve the gas production problem of the battery under high voltage. In addition, the interface layer is not easy to shrink at low temperatures, and can maintain the lithium ion transmission channel at low temperatures to improve the low temperature (such as -20°C) performance of lithium-ion batteries. The low viscosity characteristic is also conducive to the rapid migration of ions under fast charging conditions, and can support the fast charging characteristics of secondary batteries. Furthermore, compound A is a double oxygen-containing heterocyclic structure, which can complex the residual alkali on the surface of the high-nickel ternary positive electrode material to reduce the interfacial side reactions of the battery during the cycle and storage process, effectively inhibit the decomposition of the SEI film interface, and thus improve the high temperature storage and high temperature cycle performance of the secondary battery.
[0055] Although Comparative Examples 5 to 8 contain compound 7 similar to compound A, the overall performance is poor because the oxidation potential of the substance is too low and the oxidation product has poor stability. Therefore, it cannot effectively solve the problems of easy gas production and SEI film decomposition of high-nickel ternary positive electrode materials.
[0056] By comparing Example 7 with Examples 13 to 16, it can be seen that adding an auxiliary agent on the basis of compound A can further improve the high-temperature storage performance, high-temperature cycle performance, and low-temperature performance of the lithium-ion battery.
[0057] By comparing Example 2 with Examples 10 to 11, it can be seen that when the electrolyte salt is a mixture of LiPF6 and LiFSI, the comprehensive electrochemical performance of the battery is better. This is because LiFSI has better thermal stability and power characteristics, but has corrosion problems on the current collector, while LiPF6 can passivate the current collector, thereby alleviating the negative impact of LiFSI on the current collector. When LiPF6 and LiFSI are mixed, the battery performance is brought into play.
[0058] By comparing Examples 17 to 19, it can be seen that when VC / FEC mixed additives are used on the basis of a certain content of compound A, the high temperature performance and low temperature performance of the lithium-ion battery can be greatly improved, and the expansion rate is further improved. This is because VC, FEC and compound A form a multi-component interface, which further improves the electrolyte electrode interface stability and lithium ion transmission characteristics, and the battery performance is significantly improved.
[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An electrolyte comprising an electrolyte salt, an organic solvent and an additive, characterized in that: The additive includes compound A as shown in structural formula I, wherein R1~R4 are each independently C=R5 or CR6R7, R5 is an alkylene group, R6~R7 are each independently hydrogen, halogen, C1~C6 alkyl, C2~C6 alkenyl, C2~C6 alkynyl or cyano, and the viscosity of compound A is 1~3mba / cm.
2. The electrolyte according to claim 1, characterized in that R1-R4 are each independently C=CH2 or CR6R7, and R6-R7 are each independently hydrogen, C1-C3 alkyl, C2-C3 alkenyl or C2-C3 alkynyl.
3. The electrolyte according to claim 1, characterized in that The compound A is selected from at least one of compounds 1 to 6:
4. The electrolyte according to claim 1, characterized in that The mass of the compound A accounts for 0.1% to 5.0% of the total mass of the electrolyte.
5. The electrolyte according to claim 1, characterized in that The electrolyte salt includes at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethylsulfonyl imide, lithium methanesulfonate, lithium trifluoromethylsulfonate, lithium fluorosulfonate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobisoxalatophosphate, lithium bisfluorosulfonyl imide, lithium diphosphate and lithium lower aliphatic carboxylate.
6. The electrolyte according to claim 1, characterized in that The mass of the electrolyte salt accounts for 5-25% of the total mass of the electrolyte.
7. The electrolyte according to claim 1, characterized in that The organic solvent includes at least one of carbonate, carboxylate and ether compounds.
8. The electrolyte according to claim 1, characterized in that The auxiliary agent is selected from vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate, succinic anhydride, maleic anhydride, 2-methylmaleic anhydride, methyl carbonate-2-propynyl ester, tetravinylsilane, triallyl isocyanurate, hexamethylene diisocyanate, o-phenanthroline, p-phenylene diisocyanate, 2 , at least one of 4-toluene diisocyanate, N-phenylbis(trifluoromethanesulfonyl)imide, vinyl bissulfate, phenyl methanesulfonate, vinyl bissulfate, bis-spiro-propylene sulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, isocyanoethyl methacrylate, methylene disulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate and tris(vinyldimethylsilyl)phosphate.
9. A lithium ion battery, characterized in that: The invention comprises a positive electrode material, a negative electrode material and the electrolyte according to any one of claims 1 to 8.
10. The lithium ion battery according to claim 9, characterized in that The positive electrode material is LiNi x Co y Mn z M 1-x-y-z O2 or LiNi x Co y Al z M 1-x-y-z O2, where M is any one of Mg, Cu, Zn, Sn, B, Ga, Cr, Sr, V and Ti, 0.5≤x<1.0, 0 <y<1.0,0<z<1.0,0.9<x+y+z≤1.0。
Citation Information
Patent Citations
Secondary cell, electrolyte, cell pack, electronic device, electric vehicle
CN105633461A
Electrochemical device and electronic device
CN116830340A
Electrolyte additives for secondary battery and electrolyte for secondary battery including the same
KR1020180118452A
Non-aqueous electrolyte for lithium ion battery and lithium ion battery
WO2022213823A1