1, 1, 1, 5, 5, 5-hexafluoro-3-(2, 2, 2-trifluoroethoxy)-2-pentene, and use and method for production thereof
The second solution was solved by the novel compound 1,1,1,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene as an additive to the non-aqueous electrolyte solution. The problem of forming the battery electrode interface coating significantly improves the battery's cycle characteristics and capacity maintenance rate, and achieves excellent battery performance.
Patent Information
- Application Number
- CN202380036065.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-27
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art lacks effective additives for non-aqueous electrolytes, which affect the formation of electrode interface coatings and battery performance of secondary batteries.
Provided a novel compound 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, by 1,1,1,5, 5,5-hexafluoro-3-chloro-2-pentene reacts with 2,2,2-trifluoroethanol in the presence of alkali and is used as an additive for the electrolyte in the non-aqueous electrolyte.
This compound forms a high-quality coating at the interface between the positive and negative electrodes of the secondary battery, significantly improving the cycle characteristics and capacity maintenance of the battery and providing excellent battery performance.
Smart Images

Figure BDA0005099740110000021 
Figure BDA0005099740110000081 
Figure BDA0005099740110000082
Abstract
Description
Technical Field
[0001] The present invention relates to a novel compound 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, and the use and preparation method of the novel compound. Background Art
[0002] Fluoroolefins are used as solvents, detergents, foaming agents, and intermediates for functional materials, and the novel compounds of the present invention are expected to be used in the same applications. For example, in the examples of Patent Document 1, for CF 3 CH=CHOCH 2 CF 3 CF 3 CH=CHOCH 2 CF 2 CF 2 H studied the self-extinguishing property, the properties as electrolyte compound, etc. However, the novel compound of the present invention is unknown in the industry.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2021 / 064222 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] The present invention aims to provide a novel compound 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene (hereinafter sometimes referred to as "3TFEO2HFP"), and uses and a production method of the novel compound.
[0008] Solutions for solving problems
[0009] The present invention provides the following solutions. [1]
[0011] A 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene. [2]
[0013] The 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to [1], which is represented by the following formula (1).
[0014] [3]
[0016] The 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to [1], which is (E)-1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, (Z)-1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, or a combination thereof. [4]
[0018] A method for producing 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, comprising the step of reacting 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene with 2,2,2-trifluoroethanol in the presence of a base. [5]
[0020] The method according to [4], wherein the base is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide and ammonium hydroxide. [6]
[0022] The method according to [4] or [5], wherein the base is in the form of an aqueous solution and the reaction is carried out in the presence of a phase transfer catalyst. [7]
[0024] Use of 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to any one of [1] to [3] in a non-aqueous electrolyte. [8]
[0026] The use according to [7], wherein the non-aqueous electrolyte is a non-aqueous electrolyte for a secondary battery. [9]
[0028] A non-aqueous electrolyte comprising:
[0029] Electrolytes;
[0030] 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to any one of [1] to [3]; and
[0031] Non-aqueous organic solvents.
[10]
[0033] The non-aqueous electrolyte solution according to [9], wherein the electrolyte is lithium hexafluorophosphate and the non-aqueous organic solvent is a carbonate solvent.
[11]
[0035] A secondary battery comprising the nonaqueous electrolyte described in [9].
[12]
[0037] The secondary battery according to
[11] , wherein the secondary battery is a lithium ion secondary battery.
[0038] Effects of the Invention
[0039] According to the present invention, a novel compound 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene and the use and preparation method of the novel compound are provided. It is known that the novel compound is particularly useful as an additive for non-aqueous electrolytes; it can be prepared using easily available bases such as 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene, 2,2,2-trifluoroethanol, and sodium hydroxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a cross-sectional view of a stacked battery used for battery evaluation in Examples.
[0041] Figure 2 This is a graph showing the transition of the capacity retention rate in the cycle test performed in the battery evaluation of the example. DETAILED DESCRIPTION
[0042] [effect]
[0043] As shown in formula (1), the novel compound of the present invention has the following special chemical structure: trifluoromethyl and two groups with trifluoromethyl at the end (2,2,2-trifluoroethyl and 2,2,2-trifluoroethoxy) are bonded at three of the four substitution positions of the C=C double bond. The molecular weight is relatively large, 276, so the boiling point is 125-130°C / atmosphere, and it is liquid at room temperature and pressure. Since there are 9 fluorine atoms in the molecule, it is self-extinguishing. Two of the trifluoromethyl groups extending to the outside of the molecule are connected by methylene (-CH 2-) is linked to a rigid C=C double bond, so it has a relatively high degree of freedom, and the external aggressiveness of the reaction reagent to the C=C double bond is moderately restricted. The 2,2,2-trifluoroethoxy group bonded to the C=C double bond is affected by the electron-withdrawing property of the trifluoromethyl group at the end, but due to the intervention of the methylene group, it imparts moderate electron-withdrawing property to the C=C double bond compared to the trifluoromethoxy group. Therefore, the reactivity of the C=C double bond is moderately restricted. Due to such a chemical structure, the novel compound of the present invention has the following characteristics: it is a liquid at room temperature and pressure, has self-extinguishing properties, can be used in a chemically stable state, and on the other hand, can be recovered as a low molecular compound after use by cleavage of the C=C double bond and the ether bond. Due to such characteristics, the novel compound of the present invention is considered to be useful for intermediates of solvents, detergents, foaming agents and functional materials, etc. Furthermore, as described in the examples described later, the inventors have newly discovered that the novel compound of the present invention forms a high-quality coating at the interface between the positive and negative electrodes of the secondary battery, which can provide excellent battery characteristics. The electrolyte of secondary batteries usually uses non-aqueous organic solvents and adds lithium hexafluorophosphate (LiPF 6 ) as an electrolyte. The novel compound of the present invention has a trifluoromethyl group at 3 locations, and therefore has a high affinity with fluorine compounds. On the other hand, since it has a basic skeleton of a carbon chain, it also has a high affinity with non-aqueous organic solvents and can be uniformly mixed in an electrolyte. In addition, due to the conjugation of the C=C double bond and the ether bond present in the center of the molecule, the state of polarization can exist stably, and therefore has a high affinity with the interface of the positive electrode and the negative electrode, and can exist stably between these electrodes. Due to this chemical structural feature, it is considered useful as an additive for the electrolyte of a secondary battery.
[0044] [Method for producing 3TFEO2HFP]
[0045] The novel compound 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene of the present invention can be produced by reacting 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene with 2,2,2-trifluoroethanol in the presence of a base.
[0046] 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene and 2,2,2-trifluoroethanol as the raw materials are both known substances and can be easily produced by known methods or easily obtained as reagents. Trifluoroethanol can be used in a slightly excess amount relative to 1 mol of 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene, preferably in a ratio of 1 to 1.5 mol, more preferably 1 to 1.3 mol, and most preferably 1 to 1.2 mol.
[0047] Examples of the base include alkali metal hydroxides (sodium hydroxide, potassium hydroxide, etc.), hydroxides such as ammonium hydroxide, alkali metal bicarbonates or carbonates (sodium bicarbonate, sodium carbonate, etc.), inorganic bases such as metal hydrides such as alkali metal hydrides (sodium hydride, potassium hydride, etc.), alkylamines (triethylamine, tetramethylethylenediamine, N,N-diisopropylamine, etc.), 1-azabicyclo[2.2.2]octane, 1,4-diazabicyclo[2.2.2]octane (abbreviation: DABCO), 1,8-diazabicyclo[5.4.0]undec-7-ene (abbreviation: DBU), pyridine, 4-(dimethylamino)pyridine, pyrrolidine, piperidine, morpholine, and organic bases. Preferred are sodium hydroxide, potassium hydroxide, and ammonium hydroxide, and particularly preferred are sodium hydroxide (caustic soda). The base may be used in excess, preferably in a ratio of 1 to 3 moles, more preferably 1 to 2 moles, and most preferably 1 to 1.5 moles, relative to 1 mole of the raw material 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene. When the base is used in the form of an aqueous solution, the concentration of the aqueous solution is preferably 5 to 30%, more preferably 5 to 20%, and most preferably 10 to 15% based on the weight of the entire aqueous solution.
[0048] A phase transfer catalyst may be present in the reaction solution. In the case where the base used in the present invention is in the form of an aqueous solution, the reactive species is present in the aqueous phase. On the other hand, the raw materials 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene and 2,2,2-trifluoroethanol are lipophilic, and therefore are present in the oil phase and are insoluble in the aqueous phase. Therefore, if a phase transfer catalyst is used, the active species of the aqueous phase can be moved to the oil phase to promote the reaction. As a phase transfer catalyst, for example, quaternary ammonium salts such as tetrabutylammonium bromide and tetrabutylammonium chloride, quaternary phosphonium salts such as tetrabutylphosphonium chloride and tetrabutylphosphonium bromide, crown ethers such as 12-crown-4, 15-crown-5, and 18-crown-6, etc., preferably tetrabutylammonium bromide and tetrabutylammonium chloride, particularly preferably tetrabutylammonium bromide. The phase transfer catalyst is used in a ratio of preferably 0.005 to 0.1 mol, more preferably 0.01 to 0.05 mol, most preferably 0.01 to 0.02 mol, based on 1 mol of the raw material 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene.
[0049] When using a solvent, in addition to water, water-miscible solvents such as amides such as dimethylformamide (DMF), dimethyl sulfoxide (DMSO), N-methylpyrrolidone (NMP), lower alcohols such as methanol and ethanol, ethers such as tetrahydrofuran (THF), 1,4-dioxane, and acetonitrile can also be used. Even when using non-water-miscible organic solvents and water, by using the above-mentioned phase transfer catalyst, it is possible to make the reactive species exist in both the aqueous phase and the oil phase (organic solvent phase). As such an organic solvent, ether solvents such as diethyl ether, halogenated hydrocarbon solvents such as dichloromethane, aromatic hydrocarbon solvents such as benzene, toluene, and xylene, and aliphatic hydrocarbon solvents such as pentane, hexane, and octane can be used. As a solvent, preferred examples are water, DMF, and acetonitrile.
[0050] The reaction temperature is preferably -40°C to 120°C, more preferably -20°C to 60°C, more preferably -10°C to 40°C, and most preferably 0°C to 25°C. The reaction pressure may be normal pressure, and a glass reactor may be used.
[0051] [Application of 3TFEO2HFP]
[0052] As described above, the novel compound of the present invention has the following characteristics in chemical structure: it is liquid at normal temperature and pressure, has self-extinguishing property, can be used in a chemically stable state, and on the other hand, can be recovered as a low molecular compound by cleavage of C=C double bonds and ether bonds after use. Due to such characteristics, the novel compound of the present invention is considered to be useful for solvents, detergents, foaming agents, intermediates of functional materials, etc.
[0053] Furthermore, as described in the examples described later, the inventors have newly discovered that the novel compound of the present invention forms a high-quality coating at the interface of the positive and negative electrodes of the secondary battery, which can provide excellent battery characteristics. When the novel compound of the present invention is used as an additive for the electrolyte of the secondary battery, it is preferred that when the electrolyte is set to 100% by weight as a whole, it is preferably added to the electrolyte in an amount of 0.005 to 10% by weight, more preferably 0.1 to 7.5% by weight, and most preferably 1 to 5% by weight.
[0054] As a preferred compounding composition of the electrolyte solution to which the novel compound of the present invention is added, for example, the following compositions can be mentioned.
[0055] (Range of composition of electrolyte)
[0056] (1) Non-aqueous organic solvent: the remainder
[0057] As non-aqueous organic solvent, there is no particular limitation, for example, carbonate solvents such as ethylene carbonate and ethyl methyl carbonate, linear carbonate, phosphoric acid ester, cyclic ether, linear ether, lactone compound, linear ester, nitrile compound, amide compound, sulfone compound etc. can be enumerated. Among these organic solvents, from the aspect that is usually used as lithium secondary battery organic solvent, preferred carbonate solvent.
[0058] (2) Electrolyte: The amount of electrolyte is preferably 0.1 to 2 mol / L, more preferably 0.15 to 1.8 mol / L, and most preferably 0.3 to 1.2 mol / L relative to the volume of the solvent.
[0059] The electrolyte is not particularly limited, and examples thereof include lithium hexafluorophosphate (LiPF 6 ), lithium boron fluoride (LiBF 4 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 )、LiBF 3 CF 3 , LiBF 3 C 2 F 5 ,LiC 2 F 5 SO 3 ,LiC 3 F 7 SO 3 ,LiC 4 F 9 SO 3 、LiN(SO 2 F) 2 、LiN(CF 3 SO 2 ) 2 、LiN(C 2 F 5 SO 2 ) 2 、LiN(C 2 F 5 SO 2 ) 2 、LiN(CF 3 SO 2 )(CF 3 CO), LiN(CF 3 SO 2 )(C 2 F 5 SO 2 )、LiC(CF 3 SO 2 ) 3Fluorine electrolytes such as LiPF4 and LiP6 are preferred in terms of improving the safety and stability, conductivity and cycle characteristics of non-aqueous electrolytes. 6 .
[0060] (3) The novel compound of the present invention is preferably added to the electrolyte in an amount of 0.005 to 10 wt %, more preferably 0.1 to 7.5 wt %, and most preferably 1 to 5 wt %, based on 100 wt % of the entire electrolyte.
[0061] (4) Other optional additive components (fluoroethylene carbonate (FEC), vinylene carbonate (VC), lithium difluorophosphate, etc.): The amount added is small compared to the solvent or electrolyte, and is used as an additive for the purpose of improving battery performance such as film formation. When the entire electrolyte is set to 100 weight%, 0.005 to 10 weight%, more preferably 0.1 to 7.5 weight%, and most preferably 1 to 5 weight% are added to the electrolyte.
[0062] Example
[0063] [Production Example 1]
[0064] 89.3 g of 3-chloro-1,1,1,5,5,5-hexafluoro-2-pentene, 50.4 g of 2,2,2-trifluoroethanol, and 1.62 g of tetrabutylammonium bromide were introduced into a 500 mL glass three-necked flask, and 268 g of a 12.5% aqueous solution of caustic soda was added dropwise over 25 minutes. After stirring at room temperature (25°C) for 10 minutes, the formation of 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene was confirmed by NMR. After washing with water, the product was purified by distillation to obtain 76.7 g (yield 66%) of 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene with a GC purity of 99% or more. The product was analyzed and found to have an isomer ratio (E) / (Z) = 30 / 1.
[0065] [Production Example 2]
[0066] 100 g of 3-chloro-1,1,1,5,5,5-hexafluoro-2-pentene, 47.1 g of 2,2,2-trifluoroethanol, and 1.82 g of tetrabutylammonium bromide were introduced into a 500 mL glass three-necked flask, and 151 g of a 12.5% aqueous solution of caustic soda was added dropwise. After stirring at room temperature (25°C) for 12 hours, the formation of 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene was confirmed by NMR. After washing with water, the product was purified by distillation to obtain 117 g (yield 90%) of 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene with a GC purity of 99% or more. The product was analyzed and the isomer ratio (E) / (Z) was 30 / 1. The boiling point of the product (isomer mixture) is 73-76°C / 180-190 hPa, 125-130°C / atmospheric pressure.
[0067] The NMR data and GC-MS data of (E)-1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene are shown below.
[0068]
[0069] 1 H-NMR (400MHz); δ3.25 (q, JHF=9.6Hz, 2H), 4.10 (q, JHF=7.2Hz, 2H), 5.00 (q, JHF=7.6Hz, 1H).
[0070] 19 F-NMR (376MHz); δ-63.9~-64.1(m, 3F), -55.0~-55.1(m, 3F), -74.2~-74.3(m, 3F)
[0071] GC-MS m / z(%):276(CF 3 CH=C(CH 2 CF 3 )OCH 2 CF 3 ), 207(CF 3 CH=C
[0072] (CH 2 )OCH 2 CF 3 ), 193(CF 3 CH=COCH 2 CF 3 )、83(CH 2 CF 3 ).
[0073] The NMR data and GC-MS data of (Z)-1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene are shown below.
[0074]
[0075] 1 H-NMR (400 MHz); δ 3.02 (q, J HF =9.6 Hz, 2H), 4.26 (q, J HF =7.6 Hz, 2H), 5.23 (q, J HF =8.0 Hz, 1H).
[0076] 19 F-NMR (376MHz); δ-64.8~-65.0(m, 3F), -57.5~-57.6(m, 3F), -75.1~-75.2(m, 3F)
[0077] GC-MS m / z(%):276(CF 3 CH=C(CH 2 CF 3 )OCH 2 CF 3 ), 207(CF 3 CH=C
[0078] (CH 2 )OCH 2 CF 3 ), 193(CF 3 CH=COCH 2 CF 3 )、83(CH 2 CF 3 ).
[0079] [Battery evaluation]
[0080] In order to clarify that the novel compound obtained in the above manufacturing example, i.e., 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene shown in formula (1), has the effect of forming a high-quality coating, an evaluation test was performed on a non-aqueous electrolyte secondary battery using a non-aqueous electrolyte containing 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene. In addition, in order to compare the addition effect with the compound described in the example of patent document 1, a compound (CF 3 CH=CHOCH 2 CF 3 ), implement battery evaluation.
[0081] In this evaluation test, an electrolyte solution containing 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene obtained in Production Example 1 or Production Example 2 was used to prepare Figure 1 The stacked battery shown is a non-aqueous electrolyte secondary battery.
[0082] <Production steps>
[0083] [Structure of the battery used]
[0084] The cross-sectional structure of the laminated battery used in this evaluation test is shown in FIG. Figure 1 In the laminated battery, a positive electrode material 1 is applied to a positive electrode collector 2, and a positive electrode tab 3 extending from the positive electrode collector 2 can be electrically connected to a wiring from a measuring device by a fixture, a negative electrode material 5 is applied to a negative electrode collector 6, and a negative electrode tab 7 extending from the negative electrode collector 6 can be electrically connected to a wiring from a measuring device by a fixture, and a separator 4 is arranged between the positive electrode material 1 and the negative electrode material 5. Each component is a flat rectangular shape, and is arranged in layers in the order of the positive electrode collector 2, the positive electrode material 1, the separator 4, the negative electrode material 5, and the negative electrode collector 6, and is contained in a laminated outer package 8.
[0085] [Battery components used]
[0086] The positive electrode uses a lithium nickel cobalt manganese oxide (NCM111) electrode coated on an aluminum current collector, and the negative electrode uses an artificial graphite electrode coated on a nickel current collector. The thickness of the positive electrode material (electrode coating part) is 53μm, and the thickness of the negative electrode material is about 56μm. The separator is a polypropylene microporous membrane (manufactured by Celgard; trade name "Celgard#2400") cut into 5cm×6.5cm. The laminated outer package is folded in half to form 11cm×20cm. Figure 1 The stacked battery is made in a structured manner.
[0087] [Battery Assembly]
[0088] In the above-mentioned laminated battery, NCM111 is used for the positive electrode and artificial graphite is used for the negative electrode, which are cut into specified sizes (positive electrode: 4 cm×5 cm, negative electrode: 4.5 cm×5 cm) for use. The tabs for clamping the wide-mouth clamp are welded on each electrode, and a separator (5 cm×6.5 cm) is clamped between the positive electrode and the negative electrode, and placed in the laminated battery and dried at 100°C for 1 hour. Then, 0.5 mL of an electrolyte containing the compound represented by formula (1) of the present invention synthesized in Preparation Example 1 is injected into an Ar glove box, and the laminated battery is encapsulated using a vacuum sealer.
[0089] [Example 1]
[0090] In a non-aqueous solvent prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) at a volume ratio of EC:EMC=3:7, lithium hexafluorophosphate (LiPF) as an electrolyte was dissolved at a ratio of 1 mol / L. 6 , to the obtained solution, 1 wt % of the compound represented by formula (1) of the present invention is added to the solution to prepare a non-aqueous electrolyte, Figure 1 The stacked battery shown is a non-aqueous electrolyte secondary battery.
[0091] [Example 2]
[0092] In a non-aqueous solvent prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) at a volume ratio of EC:EMC=3:7, lithium hexafluorophosphate (LiPF) as an electrolyte was dissolved at a ratio of 1 mol / L. 6 , the compound represented by formula (1) of the present invention is added to the obtained solution in an amount of 5 wt % relative to the solution to prepare a non-aqueous electrolyte solution, and Figure 1 The stacked battery shown is a non-aqueous electrolyte secondary battery.
[0093] [Comparative Example 1]
[0094] In a non-aqueous solvent prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) at a volume ratio of EC:EMC=3:7, lithium hexafluorophosphate (LiPF) as an electrolyte was dissolved at a ratio of 1 mol / L. 6 .
[0095] [Comparative Example 2]
[0096] In a non-aqueous solvent prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) at a volume ratio of EC:EMC=3:7, lithium hexafluorophosphate (LiPF) as an electrolyte was dissolved at a ratio of 1 mol / L. 6 , 1 wt% CF was added to the obtained solution. 3 CH=CHOCH 2 CF 3 , prepare non-aqueous electrolyte, make Figure 1 The stacked battery shown is a non-aqueous electrolyte secondary battery.
[0097] [Comparative Example 3]
[0098] In a non-aqueous solvent prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) at a volume ratio of EC:EMC=3:7, lithium hexafluorophosphate (LiPF) as an electrolyte was dissolved at a ratio of 1 mol / L. 6 , 5 wt% of CF was added to the obtained solution. 3 CH=CHOCH2 CF 3 , prepare non-aqueous electrolyte, make Figure 1 The stacked battery shown is a non-aqueous electrolyte secondary battery.
[0099] [Measurement method]
[0100] In order to remove the initial gas, each of the non-aqueous electrolyte secondary batteries of Examples 1 to 2 and Comparative Examples 1 to 3 was charged to 30% of the theoretical capacity at 0.2C constant current at 60°C and stored for 15 hours. st Charge)
[0101] After that, the aged non-aqueous electrolyte secondary batteries of Examples 1 to 2 and Comparative Examples 1 to 3 were placed in an Ar glove box, the ends of the stacked batteries were cut off, exhaust was performed, and vacuum was again drawn with a laminator, and the stacked batteries were packaged in this state. (Exhaust)
[0102] Next, each of the non-aqueous electrolyte secondary batteries of Examples 1 to 2 and Comparative Examples 1 to 3 was charged to 4.2 V at 25°C and 0.2 C constant current, and then the charge termination C current was set to 0.02 C, and constant voltage charged to a current value of 1 / 50 of the theoretical capacity of the active material weight, and then discharged to 2.75 V at a constant current of 0.2 C. (2 nd , 3 rd Charge and discharge)
[0103] Next, each non-aqueous electrolyte secondary battery of the above-mentioned Examples 1 to 2 and Comparative Examples 1 to 3 was charged to 4.2V at 25°C and 1C constant current, and then the charge termination C current was set to 0.1C, and constant voltage charging was performed until the current value was 1 / 10 of the theoretical capacity of the active material weight, and then discharged at a constant current of 1C to 50% of the theoretical capacity.
[0104] (4 th Charge and discharge)
[0105] Then, each non-aqueous electrolyte secondary battery of Examples 1 to 2 and Comparative Examples 1 to 3 was charged to 4.2V at 45°C and 1C constant current, and then the charge termination C current was set to 0.1C, and constant voltage charged to a current value of 1 / 10 of the theoretical capacity of the active material weight, and then discharged to 2.75V at a constant current of 1C. (5 th ~Charge and discharge)
[0106] In addition, every 100 cycles, the battery was charged at a constant current of 0.2C to 4.2V, and then the charge termination C current was set to 0.1C, and the battery was charged at a constant voltage to a current value of 1 / 10 of the theoretical capacity of the active material weight, and then discharged at a constant current of 1C to 2.75V.
[0107] Based on the first (5 th ) discharge capacity D 5 , the xth discharge capacity D x (x=105, 205), the capacity retention rate (%) after the xth cycle of each nonaqueous electrolyte secondary battery of Examples 1 to 2 and Comparative Examples 1 to 3 was calculated by the following formula, and the results are shown in Table 1.
[0108] Capacity maintenance rate (%) = (D x / D 5 )×100
[0109] [Table 1]
[0110]
[0111] According to Table 1, the capacity retention rates of Examples 1 to 2 in the 105th cycle were higher than those of Comparative Examples 1 to 3, and the cycle characteristics were excellent. In the 205th cycle, the capacity retention rates of the Examples and Comparative Examples further differed, and the highest capacity retention rate was shown in Example 2. It can be said that 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene represented by formula (1) of the present invention forms a high-quality coating at the interface between the positive electrode and the negative electrode, and can provide excellent battery characteristics.
Claims
1. 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene.
2. The 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to claim 1, which is represented by the following formula (1):
3. The 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to claim 1, which is (E)-1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, (Z)-1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, or a combination thereof.
4. A method for producing 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene, comprising the step of reacting 1,1,1,5,5,5-hexafluoro-3-chloro-2-pentene with 2,2,2-trifluoroethanol in the presence of a base.
5. The method according to claim 4, wherein: The base is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, and ammonium hydroxide.
6. The method according to claim 4 or 5, wherein: The base is in the form of an aqueous solution, and the reaction is carried out in the presence of a phase transfer catalyst.
7. Use of the 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to any one of claims 1 to 3 in a non-aqueous electrolyte.
8. The use according to claim 7, wherein The non-aqueous electrolyte is a non-aqueous electrolyte for a secondary battery.
9. A non-aqueous electrolyte comprising: Electrolytes; 1,1,1,5,5,5-hexafluoro-3-(2,2,2-trifluoroethoxy)-2-pentene according to any one of claims 1 to 3; and Non-aqueous organic solvents.
10. The non-aqueous electrolyte according to claim 9, wherein The electrolyte is lithium hexafluorophosphate, and the non-aqueous organic solvent is a carbonate solvent. 11 . A secondary battery comprising the nonaqueous electrolyte according to claim 9 .
12. The secondary battery according to claim 11, wherein The secondary battery is a lithium ion secondary battery.