Solid-waste-based self-leveling mortar and preparation method thereof

By mixing industrial solid waste materials with specific additives, the existing self-leveling mortar costs and incomplete utilization of industrial solid waste are solved, and low-cost and high-performance production of solid waste-based self-leveling mortar is achieved.

CN120004582APending Publication Date: 2025-05-16REAL ESTATE CONSTR ANGANG GROUP +1

Patent Information

Application Number
CN202510118502.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-24
Publication Date
2025-05-16

AI Technical Summary

Technical Problem

The existing self-leveling mortar is costly and the production of completely replaces raw materials has not yet been achieved in the use of industrial solid waste.

Method used

Industrial solid waste materials such as granulated blast furnace slag powder, steel slag powder, industrial by-product gypsum powder, iron tailings sand and steel slag sand are used, combined with aluminate cement, high-performance water reducing agent, glue powder, calcium formate, defoaming agent and cellulose, and solid waste-based self-leveling mortar is prepared by stirring and mixing.

Benefits of technology

It has achieved the complete use of industrial solid waste materials to replace raw materials to produce self-leveling mortar, which has reduced production costs and improved the fluidity of the mortar, distribution uniformity after hardening, segregation resistance and heat conduction performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005258376510000041
    Figure BDA0005258376510000041
  • Figure BDA0005258376510000051
    Figure BDA0005258376510000051
Patent Text Reader

Abstract

The invention relates to solid waste based self-leveling mortar, which is prepared from the following ingredients in parts by weight: 197 to 217 parts of granulated blast furnace slag powder, 151 to 171 parts of steel slag powder, 105 to 125 parts of industrial byproduct gypsum powder, 390 to 410 parts of iron tailing sand, 90 to 110 parts of steel slag sand, 10 to 30 parts of aluminate cement, 1.5 to 3.5 parts of high-performance water reducing agents, 10 to 30 parts of rubber powder, 1.5 to 3.5 parts of calcium formate, 1.5 to 3.5 parts of defoaming agents and 0.2 to 0.4 part of cellulose. Industrial solid waste materials are completely used as raw materials, industrial solid waste is fully utilized, energy is saved, the environment is protected, and the production cost is low. The coating has good fluidity, is uniformly spread, and can well flow into gaps of the floor heating pipeline. And the hardened self-leveling mortar is uniformly distributed and has good segregation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of application of building material technology, and in particular to a solid waste-based self-leveling mortar and a preparation method thereof. Background Art

[0002] With the continuous advancement of construction technology, self-leveling mortar has developed rapidly due to its excellent performance. The application of industrial solid waste in self-leveling mortar can improve the performance of mortar, reduce costs, reduce resource and energy consumption, and meet the requirements of the era of low-carbon and environmental protection. In recent years, my country has achieved certain results in the research and application of solid waste in self-leveling mortar.

[0003] As an ideal new material and technology for ground construction, self-leveling materials are favored by the market due to their excellent performance and simple and fast construction methods, and have a very broad application prospect. The high cost of traditional self-leveling mortar limits its promotion and application. Applying industrial solid waste to self-leveling mortar can not only reduce costs, but also improve the performance of self-leveling mortar by utilizing certain characteristics of industrial solid waste (such as wear resistance and expansion). More importantly, it can save resources and realize resource recycling.

[0004] CN202211576850 relates to a cement-based sandless self-leveling floor material prepared from waste powder and its preparation process, wherein the waste powder is powder produced in the process of preparing aggregate from natural stone or preparing recycled aggregate from construction waste. So far, many patents on self-leveling mortar have not involved the production of self-leveling mortar completely using industrial solid waste materials instead of raw materials. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a solid waste-based self-leveling mortar and a preparation method thereof. The application of industrial solid waste to the self-leveling mortar can not only reduce costs, but also utilize the wear resistance and expansion properties of the industrial solid waste to improve the performance of the self-leveling mortar. More importantly, it can save resources and realize resource recycling.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A solid waste-based self-leveling mortar comprises the following components by weight: 197-217 parts of granulated blast furnace slag powder, 151-171 parts of steel slag powder, 105-125 parts of industrial by-product gypsum powder, 390-410 parts of iron tailings sand, 90-110 parts of steel slag sand, 10-30 parts of aluminate cement, 1.5-3.5 parts of high-performance water reducing agent, 10-30 parts of glue powder, 1.5-3.5 parts of calcium formate, 1.5-3.5 parts of defoaming agent and 0.2-0.4 parts of cellulose.

[0008] The granulated blast furnace slag powder is S95 grade granulated blast furnace slag powder.

[0009] The steel slag powder is first-grade steel slag powder.

[0010] The industrial by-product gypsum powder is industrial by-product gypsum with a fineness of 0.080 mm and a sieve residue of ≤1.0%.

[0011] The iron tailings sand has a bulk density of 1700 kg / m3 and a fineness modulus of 2.45.

[0012] The steel slag sand is fine sand with a fineness modulus of 1.6-2.2.

[0013] The high-performance water reducing agent is a powdered polycarboxylic acid-based high-performance water reducing agent.

[0014] The rubber powder is a copolymer of ethylene-vinyl acetate.

[0015] The defoamer is an organosilicon concrete defoamer.

[0016] The cellulose is hydroxypropyl methylcellulose.

[0017] A method for preparing a solid waste-based self-leveling mortar comprises the following steps:

[0018] 1) Granulated blast furnace slag powder, steel slag powder and industrial by-product gypsum powder are mixed in proportion to obtain a GC42.5 grade solid waste-based cementitious material;

[0019] 2) Aluminate cement, high-performance water reducing agent, rubber powder, calcium formate, defoaming agent and cellulose are mixed in proportion to obtain a composite functional additive;

[0020] 3) The above two materials, iron tailings sand and steel slag sand are put into a rotating mixer and stirred for 3-5 minutes to obtain a solid waste-based self-leveling mortar dry mix with uniform color.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. Use industrial solid waste materials as raw materials, make full use of industrial solid waste, save energy and protect the environment, and have low production costs.

[0023] 2. It has good fluidity, spreads evenly, and can flow well into the gaps in floor heating pipes.

[0024] 3. The hardened self-leveling mortar is evenly distributed and has good anti-segregation ability.

[0025] 4. The dense structure of self-leveling mortar is conducive to uniform upward conduction of heat and can well ensure the thermal effect.

[0026] 5. High strength, fast hardening, extremely low shrinkage, not easy to crack, delaminate or hollow.

[0027] The present invention uses industrial solid waste as the main raw material, has excellent product performance, and is a green, environmentally friendly, and low-carbon material. DETAILED DESCRIPTION

[0028] It should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit the present application. The reference to "embodiment" in this article means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] A solid waste-based self-leveling mortar comprises the following components by weight: 197-217 parts of granulated blast furnace slag powder, 151-171 parts of steel slag powder, 105-125 parts of industrial by-product gypsum powder, 390-410 parts of iron tailings sand, 90-110 parts of steel slag sand, 10-30 parts of aluminate cement, 1.5-3.5 parts of high-performance water reducing agent, 10-30 parts of glue powder, 1.5-3.5 parts of calcium formate, 1.5-3.5 parts of defoaming agent and 0.2-0.4 parts of cellulose.

[0030] The granulated blast furnace slag powder is S95 grade granulated blast furnace slag powder.

[0031] The steel slag powder is first-grade steel slag powder.

[0032] The industrial by-product gypsum powder is industrial by-product gypsum with a fineness of 0.080 mm and a sieve residue of ≤1.0%.

[0033] The iron tailings sand has a bulk density of 1700 kg / m3 and a fineness modulus of 2.45.

[0034] The steel slag sand is fine sand with a fineness modulus of 1.6-2.2.

[0035] The high-performance water reducing agent is a powdered polycarboxylic acid-based high-performance water reducing agent.

[0036] The rubber powder is a copolymer of ethylene-vinyl acetate.

[0037] The defoamer is an organosilicon concrete defoamer.

[0038] The cellulose is hydroxypropyl methylcellulose.

[0039] A method for preparing a solid waste-based self-leveling mortar comprises the following steps:

[0040] 1) mixing granulated blast furnace slag powder, steel slag powder and industrial by-product gypsum powder in proportion to obtain a GC42.5 grade solid waste-based cementitious material;

[0041] 2) Aluminate cement, high-performance water reducing agent, rubber powder, calcium formate, defoaming agent and cellulose are mixed in proportion to obtain a composite functional additive with water reducing, early strength, plasticizing, fluidizing and thickening functions;

[0042] 3) The above two materials, iron tailings sand and steel slag sand are put into a rotating mixer and stirred for 3-5 minutes to obtain a solid waste-based self-leveling mortar dry mix with uniform color.

[0043] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0044] Embodiment 1:

[0045] A method for preparing a solid waste-based self-leveling mortar, comprising:

[0046] 1. By weight, 207 parts of granulated blast furnace slag powder (S95 grade granulated blast furnace slag powder, whose indicators meet the requirements of GB / T18046-2017), 161 parts of steel slag powder (in accordance with the first-grade steel slag powder in "Steel Slag Powder for Cement and Concrete" GB / T20491-2017), and 115 parts of industrial by-product gypsum powder (industrial by-product gypsum with a fineness of 0.080 mm square hole sieve residue ≤1.0% in "Industrial By-product Gypsum for Cement" GB / T21371-2019) are mixed and stirred to obtain GC42.5 grade solid waste-based cementitious material (assessed in accordance with "Solid Waste-based Cementitious Material" T / CECS10400-2024); the above three raw materials are all solid waste from the metallurgical industry.

[0047] 2. Mix 20 parts of aluminate cement (A600 type), 2.5 parts of high-performance water reducer (powdered polycarboxylic acid-based high-performance water reducer produced by Shenyang Shengxinyuan Admixture Co., Ltd.), 20 parts of rubber powder (redispersible latex powder), 2.5 parts of calcium formate, 2.5 parts of defoamer (D508 type silicone concrete defoamer), and 0.3 parts of cellulose (hydroxypropyl methylcellulose HPMC-400 distributed by Guangdong Longhu Technology Co., Ltd.) to obtain a composite multifunctional additive.

[0048] 3. Put the above two materials and 400 parts of iron tailings sand (tailings produced by Anqian Mine, with a bulk density of 1700 kg / m3 and a fineness modulus of 2.45) and 100 parts of steel slag sand (fine sand in accordance with the "Steel Slag Sand for Ordinary Premixed Mortar" YB / T4201-2009, with a fineness modulus of 1.6-2.2) into a rotating mixer and stir for 3-5 minutes to obtain a solid waste-based self-leveling mortar dry mix with uniform color; the iron tailings sand is the tailings produced by Anqian Mine, and the steel slag sand is the tailings from steelmaking. Both materials are solid waste from the metallurgical industry.

[0049] The properties of the solid waste-based self-leveling mortar dry mix are shown in Table 1:

[0050]

[0051] Embodiment 2:

[0052] A method for preparing a solid waste-based self-leveling mortar, comprising:

[0053] 1. By weight, 200 parts of granulated blast furnace slag powder (S95 grade granulated blast furnace slag powder, whose indicators meet the requirements of GB / T18046-2017), 170 parts of steel slag powder (a-grade steel slag powder in accordance with GB / T20491-2017 "Steel Slag Powder for Cement and Concrete"), and 120 parts of industrial by-product gypsum powder (industrial by-product gypsum with a fineness of 0.080 mm square hole sieve residue ≤1.0% in GB / T21371-2019 "Industrial By-product Gypsum for Cement") are mixed and stirred to obtain GC42.5 grade solid waste-based cementitious material; the above three raw materials are all solid waste from the metallurgical industry.

[0054] 2. Mix 15 parts of aluminate cement (A600 type), 2.5 parts of high-performance water reducer (powdered polycarboxylic acid-based high-performance water reducer produced by Shenyang Shengxinyuan Admixture Co., Ltd.), 25 parts of rubber powder (redispersible latex powder), 3 parts of calcium formate, 1.8 parts of defoamer (D508 type silicone concrete defoamer), and 0.35 parts of cellulose (hydroxypropyl methylcellulose HPMC-400 distributed by Guangdong Longhu Technology Co., Ltd.) to obtain a composite multifunctional additive.

[0055] 3. Put the above two materials and 405 parts of iron tailings sand (tailings produced by Anqian Mine, with a bulk density of 1700 kg / m3 and a fineness modulus of 2.45) and 105 parts of steel slag sand (fine sand in accordance with the "Steel Slag Sand for Ordinary Premixed Mortar" YB / T4201-2009, with a fineness modulus of 1.6-2.2) into a rotating mixer and stir for 3-5 minutes to obtain a solid waste-based self-leveling mortar dry mix with uniform color.

[0056] The properties of the solid waste-based self-leveling mortar dry mix are shown in Table 2:

[0057]

[0058] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A solid waste-based self-leveling mortar, characterized in that: Its components include, by weight: 197-217 parts of granulated blast furnace slag powder, 151-171 parts of steel slag powder, 105-125 parts of industrial by-product gypsum powder, 390-410 parts of iron tailings sand, 90-110 parts of steel slag sand, 10-30 parts of aluminate cement, 1.5-3.5 parts of high-performance water reducing agent, 10-30 parts of rubber powder, 1.5-3.5 parts of calcium formate, 1.5-3.5 parts of defoaming agent and 0.2-0.4 parts of cellulose.

2. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The granulated blast furnace slag powder is S95 grade granulated blast furnace slag powder.

3. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The steel slag powder is first-grade steel slag powder.

4. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The industrial by-product gypsum powder is industrial by-product gypsum with a fineness of 0.080 mm and a sieve residue of ≤1.0%.

5. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The iron tailings sand has a bulk density of 1700 kg / m3 and a fineness modulus of 2.

45.

6. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The steel slag sand is fine sand with a fineness modulus of 1.6-2.

2.

7. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The high-performance water reducing agent is a powdered polycarboxylic acid-based high-performance water reducing agent.

8. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The rubber powder is a copolymer of ethylene-vinyl acetate.

9. The solid waste-based self-leveling mortar according to claim 1, characterized in that: The defoamer is an organosilicon concrete defoamer.

10. The method for preparing solid waste-based self-leveling mortar according to claim 1, characterized in that: The steps include: 1) Granulated blast furnace slag powder, steel slag powder and industrial by-product gypsum powder are mixed in proportion to obtain a GC42.5 grade solid waste-based cementitious material; 2) Aluminate cement, high-performance water reducing agent, rubber powder, calcium formate, defoaming agent and cellulose are mixed in proportion to obtain a composite functional additive; 3) The above two materials, iron tailings sand and steel slag sand are put into a rotating mixer and stirred for 3-5 minutes to obtain a solid waste-based self-leveling mortar dry mix with uniform color.

Citation Information

Patent Citations

  • Cement-based sand-free self-leveling terrace material prepared from waste powder and preparation process of cement-based sand-free self-leveling terrace material

    CN115819041A

Cited By

  • Steel slag wear-resistant sand as well as preparation method and construction method thereof

    CN121517126A