Potassium titanate lithium battery negative electrode material with plate-shaped tunnel structure as well as preparation method and application of potassium titanate lithium battery negative electrode material

By treating the layered potassium iron titanate with acid solution and heat treatment, a plate-shaped KxFeyTi8-yO16 material with exposed (001) crystal surface was prepared, which solved the problem of poor electrochemical performance of existing materials and achieved higher specific capacity and cycle stability.

CN120072919AActive Publication Date: 2025-05-30NORTHWESTERN POLYTECHNICAL UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202510170720.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-17
Publication Date
2025-05-30
Estimated Expiration
2045-02-17

AI Technical Summary

Technical Problem

The existing KxFeyTi8-yO16 material is mainly rod-shaped, and it fails to effectively expose the (001) tunnel surface that is conducive to lithium ion migration, resulting in poor electrochemical performance.

Method used

The plate-shaped KxFeyTi8-yO16 material was prepared by treating the layered iron potassium titanate K0.4H0.3Fe0.7Ti1.3O4 in a low-concentration acid solution and then undergoing heat treatment, and the plate-shaped KxFeyTi8-yO16 material was prepared, which exposed the (001) crystal surface was conducive to lithium ion migration.

Benefits of technology

The prepared plate-shaped KxFeyTi8-yO16 material exhibits better electrochemical properties, including higher specific capacity and better cycle stability, and is suitable for negative electrode materials for lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120072919A_ABST
    Figure CN120072919A_ABST
Patent Text Reader

Abstract

The invention relates to the field of material preparation, and discloses a potassium titanate lithium battery negative electrode material with a plate-shaped tunnel structure as well as a preparation method and application thereof, the preparation method comprises the following steps: treating layered potassium iron titanate K < 0.4 > H < 0.3 > Fe < 0.7 > Ti < 1.3O4 > with a low-concentration acid solution, filtering, washing and drying to obtain layered potassium iron titanate K < 0.4-m > H < 0.3 + m > Fe < 0.7 > Ti < 1.3O4 > (0 lt; mlt; mlt; 0.4); the preparation method comprises the following steps: carrying out heat treatment on layered titanic acid K < 0.4-m > H < 0.3 + m > Fe < 0.7 > Ti < 1.3O4 > to obtain plate-shaped K < x > Fe < y > Ti < 8-y > O < 16 > (wherein x is equal to 0.1-1.2, and y is equal to 0.5-6.2) with an exposed (001) crystal face and a tunnel structure. According to the preparation method, layered K0. 4H0. 3Fe0. 7Ti1. 3O4 is used as a precursor, a soft chemical in-situ topological transformation reaction is utilized, the heat treatment temperature is controlled, plate-shaped KxFeyTi8-yO16 particles are prepared and are small in particle size and narrow in distribution, compared with reported molten salt methods and coprecipitation methods, the KxFeyTi8-yO16 prepared through the technology is small in particle size and controllable in morphology and microstructure, the preparation process is simple, and the preparation method is suitable for industrial production. Energy consumption is low, repeatability is high, and industrial production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material preparation, and particularly to a lithium titanate negative electrode material with a plate-like tunnel structure, a preparation method thereof, and an application thereof. Background Art

[0002] Lithium ion batteries have been widely used in mobile devices, electric vehicles and other fields due to their high specific capacity and good cycle stability. The electrochemical performance of lithium ion batteries mainly depends on their electrode materials, including the positive electrode and the negative electrode. In recent years, researchers have made many efforts to improve battery materials so that they can be applied to electric vehicles. Conventional lithium ion batteries use graphite as the negative electrode material because of the abundant reserves of graphite. However, graphite has poor performance at high charge and discharge rates and there are safety problems caused by the formation of lithium dendrites due to the low lithium ion intercalation potential. One way to solve this problem is to find carbon-based materials with both high rate performance and safety performance to replace it. Titanium-based materials, such as TiO 2 and Li 4 Ti 5 O 12 , have good cycle stability and safety. The tunnel structure of K x Fe y Ti 8-y O 16 is a zero-strain material and has application potential as a lithium ion battery. At present, the synthesis methods of K x Fe y Ti 8-y O 16 mainly include the molten salt method and the solid phase method. However, the currently obtained K x Fe y Ti 8-y O 16 are all in rod-like morphology, and the (001) tunnel plane that is beneficial to lithium ion migration is not exposed. Summary of the Invention

[0003] In order to overcome the defects existing in the above-mentioned prior art, the purpose of the present invention is to provide a preparation method and an application of a lithium titanate negative electrode material with a plate-like tunnel structure. The K x Fe y Ti 8-y O 16 prepared by this method has small particle size, controllable morphology and microstructure, high specific capacity when applied to the battery, and controllable ion exchange, and can selectively exchange part of the K + in the precursor interlayer. Experiments show that the K x Fe y Ti 8-y O 16 prepared by this method exhibits better electrochemical performance compared with the rod-like structure.

[0004] To achieve the above object, on the one hand, the present invention provides a preparation method of a potassium titanate lithium battery anode material with a plate-like tunnel structure, which includes the following steps: treating potassium iron titanate K 0.4 H 0.3 Fe 0.7 Ti 1.3 O 4 with a low-concentration acid solution, filtering, washing, and drying to obtain potassium titanate K 0.4-m H 0.3+m Fe 0.7 Ti 1.3 O 4 (0 < m < 0.4); then heat-treating potassium titanate K 0.4-m H 0.3+m Fe 0.7 Ti 1.3 O 4 at 400 - 800 °C to obtain plate-like K x Fe y Ti 8-y O 16 (where x = 0.1 - 1.2, y = 0.5 - 6.2) with a tunnel structure exposing the (001) crystal plane, which is the potassium titanate lithium battery anode material with a plate-like tunnel structure.

[0005] As a further preferred technical solution of the present invention, the acid solution is at least one of acetic acid, hydrochloric acid, and sulfuric acid solution.

[0006] As a further preferred technical solution of the present invention, the concentration of the acid solution is 0.1 - 2 mol / L.

[0007] According to another aspect of the present invention, the present invention also provides a potassium titanate lithium battery anode material with a plate-like tunnel structure, which is prepared by the above method.

[0008] As a further preferred technical solution of the present invention, the length of the potassium titanate lithium battery anode material is 1 - 2 μm, and the thickness is 20 - 50 nm.

[0009] According to yet another aspect of the present invention, the present invention also provides an application of a potassium titanate lithium battery anode material with a plate-like tunnel structure in a lithium-ion battery.

[0010] As a further preferred technical solution of the present invention, the potassium titanate lithium battery anode material, acetylene black, and polyvinylidene fluoride are mixed in a mass ratio of 70 - 80:10 - 15:5 - 10, and after adding the solvent N-methylpyrrolidone, they are ground into a slurry and uniformly coated on a conductive metal sheet as the anode of a lithium-ion battery.

[0011] Compared with the prior art, the present invention has the following beneficial effects:

[0012] The preparation method provided by the present invention uses layered K 0.4 H 0.3 Fe 0.7 Ti 1.3 O 4 as a precursor, and through a soft chemical in-situ topological transformation reaction, by controlling the heat treatment temperature, plate-shaped K x Fe y Ti 8-y O 16 particles are prepared. The particles have small particle size and narrow distribution (the length is about 1-2 μm, and the thickness is 20-50 nm); compared with the reported molten salt method and co-precipitation method, the K x Fe y Ti 8- y O 16 prepared by the technology of the present invention has small particle size, controllable morphology and microstructure, and its preparation process is simple, with low energy consumption and high repeatability, which is conducive to industrial production. The plate-shaped K x Fe y Ti 8-y O 16 particles can be used as the negative electrode material of a lithium ion battery and exhibit good electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The present invention will be further described in detail below with reference to the drawings and specific embodiments.

[0014] Figure 1 XRD patterns of the potassium titanate lithium negative electrode materials obtained in Examples 1-4 and Comparative Example 1: (a) plate-shaped particles; (b) rod-shaped particles.

[0015] Figure 2 SEM images of the plate-shaped particles obtained after heat treatment at different temperatures in Examples 1-4: (a) 500 °C; (b) 600 °C; (c) 700 °C; (d) 800 °C.

[0016] Figure 3 Characterization of the obtained crystal structures: (a-c) plate-shaped particles (Example 1); (d-f) rod-shaped particles (Example 5).

[0017] Figure 4 Cycling performance graphs of the plate-shaped and rod-shaped particles at a current density of 100 mA / g for 100 cycles.

[0018] The implementation, functional features and advantages of the present invention will be further described with reference to the embodiments and the drawings. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0019] The following is a detailed description of the specific embodiments of the present invention in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only for the purpose of illustrating and explaining the present invention, and are not intended to limit the present invention.

[0020] Unless otherwise defined, the technical terms used in the following embodiments have the same meanings as commonly understood by those skilled in the art to which the present invention pertains. The test reagents used in the following embodiments are all conventional biochemical reagents unless otherwise specified; the experimental methods are all conventional methods unless otherwise specified.

[0021] The potassium iron titanate K 0.4 H 0.3 Fe 0.7 Ti 1.3 O 4 used in the present invention can be prepared by the hydrothermal preparation method of a kind of iron-containing potassium titanate platelet particles disclosed in the Chinese patent with the application number 201710743855.7.

[0022] The potassium iron titanate K 0.4 H 0.3 Fe 0.7 Ti 1.3 O 4 adopted in the following embodiments is prepared by the following method, specifically as follows:

[0023] 5 g of titanium dioxide, 16.87 g of iron nitrate nonahydrate, and 20 g of potassium hydroxide are added to 18 mL of water, mixed evenly, transferred to a hydrothermal autoclave, hydrothermally treated at 250 °C for 24 h, and then the obtained product is filtered, washed, and dried at room temperature to obtain potassium iron titanate K 0.4 H 0.3 Fe 0.7 Ti 1.3 O 4 .

[0024] Example 1

[0025] The preparation method of the potassium titanate lithium battery anode material provided in this example and the lithium ion battery using this potassium titanate lithium battery anode material is specifically as follows:

[0026] 1) 0.2 g of potassium iron titanate K 0.4 H 0.3 Fe 0.7 Ti 1.3 O 4 is added to a 0.5 mol / L acetic acid solution, stirred at room temperature for 12 h, and after the reaction is completed, it is filtered, washed, and dried to obtain layered K 0.2 H 0.5 Fe 0.7 Ti 1.3 O 4, then calcine the product in a muffle furnace at 500 °C for 3 h to obtain the lithium titanate negative electrode material in the form of plate-like K 0.5 Fe 2.2 Ti 5.8 O 16 particles, with a length of about 1 - 2 μm and a thickness of 20 - 50 nm, and the plate-like surface is smooth.

[0027] 2) Mix the plate-like K 0.5 Fe 2.2 Ti 5.8 O 16 particles, acetylene black, and polyvinylidene fluoride in a mass ratio of 70:20:10, add N-methylpyrrolidone and then grind, and evenly coat it on a copper sheet as the negative electrode of the lithium-ion battery. Then, use metallic lithium as the positive electrode and 1 mol / L LiPF 6 in the EC + DEC + DMC (EC / DEC / DMC = 1 / 1 / 1, v / v / v) solution to assemble the battery in a glove box. After the battery assembly is completed, use an electrochemical workstation to test the performance of the battery such as rate and cycle.

[0028] Example 2

[0029] Based on Example 1, the difference from Example 1 is only that: replace the calcination temperature in the muffle furnace with 600 °C, and keep other operations and processes the same. The lithium titanate negative electrode material obtained in Example 2 is plate-like K 0.8 Fe 2.2 Ti 5.8 O 16 , with a length of about 1 - 2 μm and a thickness of 20 - 50 nm, and the plate-like surface is smooth.

[0030] Example 3

[0031] Based on Example 1, the difference from Example 1 is only that: replace the calcination temperature in the muffle furnace with 700 °C, and keep other operations and processes the same. The lithium titanate negative electrode material obtained in Example 3 is plate-like KFe 2.5 Ti 5.5 O 16 , with a length of about 1 - 2 μm and a thickness of 20 - 50 nm, the plate-like surface is smooth, the plate-like surface is rough, with obvious particles, and it is a mesocrystal composed of nanocrystals.

[0032] Example 4

[0033] Based on Example 1, the difference from Example 1 is only that: replace the calcination temperature in the muffle furnace with 800 °C, and keep other operations and processes the same. The lithium titanate negative electrode material obtained in Example 3 is plate-like K 1.2 Fe 1.8 Ti 6.2O 16 , with a length of about 1 - 2 μm and a thickness of 20 - 50 nm.

[0034] Comparative Example 1

[0035] As a control experiment for Examples 1 - 4, the specific method is as follows:

[0036] 1) Add 2 g of layered potassium iron titanate K 0.4 H 0.3 Fe 0.7 Ti 1.3 O 4 to a 4 mol / L hydrochloric acid solution, stir at room temperature for 12 h. After the reaction is completed, filter, wash, and dry to obtain rod-shaped K 1.5 Fe 1.5 Ti 5.5 O 16 particles, with a length of about 1 - 2 μm and a diameter of 20 - 50 nm.

[0037] 2) Mix rod-shaped K 1.5 Fe 1.5 Ti 5.5 O 16 particles, acetylene black, and polyvinylidene fluoride in a mass ratio of 70:20:10, add N-methylpyrrolidone and then grind, and evenly coat it on a copper sheet as the negative electrode of a lithium-ion battery. Then, use metallic lithium as the positive electrode and 1 mol / L LiPF 6 in EC + DEC + DMC (EC / DEC / DMC = 1 / 1 / 1, v / v / v) solution to assemble the battery in a glove box. After the battery assembly is completed, use an electrochemical workstation to test the performance of the battery such as rate and cycle.

[0038] The detailed comparison between Examples 1 - 4 and Comparative Example 1 is shown in Table 1.

[0039] Table 1

[0040]

[0041] Note: The K ion content of the plate-like particle products obtained in Examples 1 - 4 increases in sequence, that is, the tunnels are gradually occupied by K ions.

[0042] See Figure 1 , which is the XRD pattern of the plate-like K x Fe y Ti 8-y O 16 particles prepared in Examples 1 - 4. Figure 1(a) XRD of plate-like particles obtained by heat treatment at different temperatures (500 - 800 °C correspond to Examples 1 - 4 respectively). It can be seen from the figure that as the heat treatment temperature increases, the relative intensities of the diffraction peaks corresponding to 2θ = 12.5 degrees and 17.5 degrees gradually decrease, indicating that the K ion content in the tunnel increases, and the K tunnel gradually approaches the filled state. Figure (b) shows the K of the rod-like particles obtained after treatment with 4 mol / L hydrochloric acid in Comparative Example 1 1.5 Fe 1.5 Ti 5.5 O 16 XRD pattern, and its diffraction peaks are similar to those of Figure 1 (a) at 800 °C, indicating that the K ions in the rod-like particle tunnels are in the filled state.

[0043] See Figure 2 , which are SEM photos of K x Fe y Ti 8-y O 16 plate-like particles heat-treated at different temperatures prepared in Examples 1 - 4. It can be clearly seen from the figure that the morphology of the K x Fe y Ti 8-y O 16 particles is plate-like, with a length of about 1 - 2 μm and a thickness of 20 - 50 nm. The surface of the plate is smooth after heat treatment at 500 - 700 °C, and particles appear on the surface after heat treatment at 800 °C, indicating that the plate-like particles are mesocrystals composed of nanocrystals.

[0044] See Figure 3 , and from Figure 3 (c), two sets of crystal planes of the plate-like particles can be observed, namely (2 - 20) and (0 - 40). According to the zone law, the crystal axis parallel to the transmitted incident electron beam is

[001] , so the exposed crystal plane can be obtained as (001); similarly, for the (200) and (501) crystal planes of the rod-like particles in Figure 3 (c), according to the zone law, the crystal axis parallel to the transmitted incident electron beam is

[010] , so the exposed crystal plane can be obtained as (010).

[0045] See Figure 4 , Figure 4 is for K 0.5 Fe 2.2 Ti 5.8 O 16 plate-like particles (Example 1) and K 1.5 Fe 1.5 Ti 5.5 O 16Cycling curve of rod-shaped particles (Comparative Example 1) at a current density of 100 mA g -1 After 100 cycles, the specific capacity of the plate-like particles is 300 mAh / g, while that of the rod-shaped particles is only 100 mAh / g. It can be seen that the plate-like particles exhibit a higher specific capacity than the rod-shaped particles. The electrochemical performance of the plate-like particles exposing the (001) crystal plane is superior to that of the rod-shaped particles exposing the (010) crystal plane because the crystal plane exposed by the plate-like particles corresponds to the tunnel plane, which is beneficial to the migration of lithium ions.

[0046] Although the specific embodiments of the present invention have been described above, those skilled in the art should understand that these are only examples. Various changes or modifications can be made to these embodiments without departing from the principle and essence of the present invention. The protection scope of the present invention is only defined by the appended claims.

Claims

1. A method for preparing a potassium lithium titanate negative electrode material with a plate-like tunnel structure, characterized in that: The following steps are involved: After treating potassium iron titanate K 0.4 H 0.3 Fe 0.7 Ti 1.3 O4 with a low-concentration acid solution, filtering, washing, and drying, potassium titanate K 0.4-m H 0.3+m Fe 0.7 Ti 1.3 O4 (0 < m < 0.4) is obtained; then potassium titanate K 0.4-m H 0.3+m Fe 0.7 Ti 1.3 O4 is heat-treated at 400 - 800 °C to obtain plate-like K x Fe y Ti 8-y O 16 (where x = 0.1 - 1.2, y = 0.5 - 6.2), which is the lithium titanate anode material with a plate-like tunnel structure.

2. The method for preparing a plate-shaped tunnel structured potassium lithium titanate negative electrode material according to claim 1, characterized in that: The acid solution is at least one of acetic acid, hydrochloric acid and sulfuric acid solution.

3. The method for preparing the plate-shaped tunnel structured potassium lithium titanate negative electrode material according to claim 1, characterized in that: The concentration of the acid solution is 0.1-2 mol / L.

4. A potassium lithium titanate negative electrode material with a plate-like tunnel structure, characterized in that: The method is prepared by any one of claims 1 to 3.

5. The plate-shaped tunnel structured potassium lithium titanate negative electrode material according to claim 4, characterized in that: The length of the potassium titanate lithium negative electrode material is 1 to 2 μm, and the thickness is 20 to 50 nm.

6. Use of the plate-shaped tunnel structured potassium lithium titanate negative electrode material according to claim 4 in a lithium ion battery.

7. The use according to claim 6, characterized in that: Potassium titanate lithium battery negative electrode material, acetylene black, and polyvinylidene fluoride are mixed in a mass ratio of 70-80:10-15:5-10, and after adding solvent N-methylpyrrolidone, they are ground into slurry, and evenly coated on a conductive metal sheet as the negative electrode of the lithium ion battery.

Citation Information

Patent Citations

  • Preparation method of flaky potassium hexatitanate

    CN102390864A

  • Preparation method of three-dimensional rod-like potassium titanate material

    CN112018355A

  • Resin composition

    JP1992325552A

  • Production of phombic layered titanic acid plate crystal represented by hxmyti2-yo4-nh2o

    JP1993229900A

  • Layered titanic acid, lamellar titanic acid, lamellar titanium oxide and method for producing lamellar titanic acid

    US20040234447A1