A secondary battery and power device

By introducing halocarboxylic acid esters and additives with specific structures into the electrolyte and using a cathode current collector containing nitrogen, the corrosion problem of lithium cobalt oxide cathode materials under high voltage was solved, thereby improving the cycle performance and stability of the battery.

CN120199896BActive Publication Date: 2026-11-17ZHEJIANG LIWINON ELECTRONIC TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510342662.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-21
Publication Date
2026-11-17
Estimated Expiration
2045-03-21

AI Technical Summary

Technical Problem

In existing technologies, the side reactions between lithium cobalt oxide cathode materials and electrolytes under high voltage lead to corrosion problems, affecting cycle performance. How to reduce the degree of corrosion and rationally design the cathode current collector are technical problems that urgently need to be solved.

Method used

A positive electrode current collector containing nitrogen elements (such as Zn, Ni, Cr, Ca, Ti) is used, and halocarboxylic acid esters and additives with specific structures are added to the electrolyte. By controlling the proportion of electrolyte components, the electrochemical characteristics of the electrolyte and current collector are optimized, and side reactions and corrosion effects are reduced.

Benefits of technology

It effectively reduces corrosion of the current collector, improves the high-temperature cycle performance and capacity retention of the battery, reduces the formation of microcracks and Al dissolution pits, and ensures the adhesion between the material and the current collector.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

This invention discloses a secondary battery and an electrical device, relating to the field of battery technology. The invention provides a secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte; the positive electrode current collector contains nitrogen (N) element, which includes at least one of Zn, Ni, Cr, Ca, and Ti; the secondary battery satisfies the following relationships: 1 ≤ (X+50) / (P+10*Q) ≤ 25, and 25 ≤ X ≤ 500, 3 ≤ P ≤ 50, 0.01 ≤ Q ≤ 5; where P is the weight percentage of the compound with structure A in the electrolyte; Q is the weight percentage of the compound with structure B in the electrolyte; and X is the content of nitrogen (N) element in the positive electrode current collector, in ppm. The elements in the positive electrode current collector of this invention are strongly correlated with the first solvent A and additive B; under the above selection, the secondary battery performance is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and in particular to a secondary battery and an electrical device. Background Technology

[0002] Lithium cobalt oxide (LiCoO2) is a highly attractive cathode material. Its reversible capacity can increase to 185 mAh / g and 220 mAh / g at 4.5V and 4.6V, respectively. However, high voltage brings serious problems, such as the oxidative decomposition of traditional carbonate electrolytes, leading to oxygen release and CEI degradation in lithium cobalt oxide materials. Cyclic carbonate solvents undergo dehydrogenation reactions at high potentials, resulting in CH4 breakage. This process triggers the formation and accumulation of HF, which, in addition to corroding the cathode material and causing the dissolution of TM ions, also leads to significant corrosion of the cathode current collector at high voltages. This is because the current collector inevitably has some microscopic defects during the manufacturing process, where the electrolyte locally concentrates HF at these defect sites. - HF species can further corrode the current collector, continuously fluorinating the original Al2O3 layer at defect sites to form AlF3 and LiF. This causes the defect area of ​​the current collector to become brittle, resulting in microcracks and Al dissolution pits in the later stages of the cycle, affecting the adhesion to the current collector and causing the cycle capacity to continuously decline.

[0003] Therefore, how to further reduce the side reactions between the high-voltage cathode and the electrolyte, reduce the degree of corrosion, and how to make the positive electrode current collector more corrosion resistant through reasonable design are technical problems that urgently need to be solved by those skilled in the art. Summary of the Invention

[0004] Based on this, the purpose of the present invention is to overcome the shortcomings of the prior art and provide a secondary battery and an electrical device.

[0005] To achieve the above objectives, in the first aspect of this application, the technical solution adopted by this application is: a secondary battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte;

[0006] The positive electrode current collector contains nitrogen element, which includes at least one of Zn, Ni, Cr, Ca, and Ti.

[0007] The electrolyte comprises an organic solvent, a lithium salt, and an additive. The organic solvent comprises a first solvent and a second solvent. The first solvent is a halocarboxylic acid ester, which is a compound represented by structural formula A. The second solvent is at least one of a carbonate compound, a non-halocarboxylic acid ester compound, an ether compound, and a nitrile compound. The additive comprises a compound represented by structural formula B.

[0008]

[0009] In Formula A, R1 and R2 are each independently selected from one of the following: halogen atoms, C1-C10 alkyl groups, and C1-C10 haloalkyl groups; and Formula A contains at least one halogen atom; in Formula B, R3, R4, R5, R6, and R7 are each independently selected from the following: H atoms, halogen atoms, and the number of carbon atoms.

[0010] ≤3 halogenated or non-halogenated alkyl or olefinic groups, One or more of the following; and formula B contains at least one halogen atom;

[0011] The secondary battery satisfies the following relationships: 1≤(X+50) / (P+10*Q)≤25, and 25≤X≤500, 3≤P≤50, 0.01≤Q≤5;

[0012] Where P is the weight percentage of the compound represented by structural formula A in the electrolyte;

[0013] Q represents the weight percentage of the compound represented by structural formula B in the electrolyte.

[0014] X represents the nitrogen content in the positive electrode current collector, expressed in ppm.

[0015] As an embodiment of this application, the halogen atom is at least one of fluorine, chlorine, bromine, and iodine.

[0016] As an embodiment of this application, structural formula A includes at least one of the following compounds:

[0017]

[0018] As an embodiment of this application, structural formula B includes at least one of the following compounds:

[0019]

[0020] As an embodiment of this application, the secondary battery satisfies the following relationship: 5≤(X+50) / (P+10*Q)≤25, and 50≤X≤200, 5≤P≤30, 0.1≤Q≤2.

[0021] As an embodiment of this application, the positive current collector further contains aluminum; after the secondary battery is discharged, the aluminum content in the electrolyte is E, in ppm, which satisfies 80≤E≤210.

[0022] As an embodiment of this application, the N element contains Zn and / or Ni, and the mass percentage of the Zn and / or Ni elements, based on the total N element content, is F, which satisfies F≥60%.

[0023] As an embodiment of this application, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiDFP), lithium difluorobis(oxalate) phosphate (LiODFP), lithium tetrafluorooxalate phosphate (LiOTFP), lithium bis(oxalate) borate (LiBOB), lithium difluorobis(oxalate) borate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium 4,5-dicyano-2-(trifluoromethyl)isoimidazolium (LiTDI).

[0024] As an embodiment of this application, the additive further includes at least one of the following: 1,3-propanesulfonate lactone (PS), lithium difluorophosphate (LiDFP), lithium difluorobis(oxalate) phosphate (LiODFP), lithium tetrafluorooxalate phosphate (LiOTFP), lithium bis(oxalate) borate (LiBOB), lithium difluorobis(oxalate) borate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium 4,5-dicyano-2-(trifluoromethyl)isoimidazolium (LiTDI), sulfate ester compounds, and nitrile compounds.

[0025] As an embodiment of this application, the nitrile compound, as an additive, includes at least one of succinic acid, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexanetrionitrile, glyceryltrionitrile, adiponitrile, heptanonitrile, octanilide, anonadionitrile, and sebacate; the sulfate ester compound includes at least one of vinyl sulfate and fluorovinyl sulfate.

[0026] As an embodiment of this application, the carbonate compound of the second solvent includes at least one selected from ethylene carbonate, fluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, vinylene carbonate, fluoroethyleneene carbonate, dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, and diphenyl carbonate; the non-halogenated carboxylic acid ester compound of the second solvent includes methyl formate, ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, and methyl propionate. The second solvent comprises at least one of the following: ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, and butyl butyrate; the ether compound of the second solvent comprises at least one of ethylene glycol dimethyl ether, 1,3-dioxolane, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether; and the nitrile compound of the second solvent comprises at least one of succinic anionibacterium, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexanetrionitrile, glycerol trionitrile, adiponitrile, heptanonitrile, octanilide, nonadionitrile, and sebacate.

[0027] As an embodiment of this application, the lithium salt has a mass percentage content of 8-25% based on the mass percentage of the electrolyte, the additive has a mass percentage content of 0.01-15%, and the second solvent has a mass percentage content of 10-85%.

[0028] As an embodiment of this application, the negative electrode sheet includes a negative electrode material, which includes at least one of lithium metal, graphite, silicon-oxygen composite material and silicon-carbon composite material.

[0029] A third aspect of this application provides an electrical device including the aforementioned secondary battery.

[0030] Compared to existing technologies, the beneficial effects of this invention are as follows: By introducing compounds represented by structural formulas A and B into the electrolyte, which exhibit electrochemical properties strongly correlated with the current collector characteristic elements in the positive electrode film, the first solvent A has a lower HOMO value, which can improve the oxidation resistance of the electrolyte bulk, reduce the decomposition of solvent and lithium salt on the positive electrode side, and further reduce the enrichment of by-products at current collector defects. Additive B has a higher HOMO value, and after halogenation, it can reduce the electron cloud density of the pyridine group in the molecular structure, lower the desolvation energy barrier, preferentially form a protective film on the positive electrode material compared to the solvent, regulate the dehydrogenation process of the carbonate solvent, and reduce the local concentration of F in the current collector. - Or HF species, which can reduce the corrosive effect on the current collector.

[0031] In the positive electrode current collector, the selection of different elements has varying degrees of improvement on the corrosion resistance and ductility of the current collector. Specifically, corrosion-resistant elements include Zn, Ni, and Cr. Zn can form a protective layer or metallic phase, improving corrosion resistance; Ni, as a stabilizer, is beneficial for forming high-melting-point intergranular compounds, inhibiting pitting corrosion; Cr is beneficial for forming an oxide film to inhibit corrosion. In addition, ductility-enhancing elements include Ca and Ti, both of which can refine grains and improve mechanical ductility. Extensive experimental data from researchers have shown that when nitrogen (N) contains both corrosion-resistant and ductility-enhancing elements, and when the total amount of corrosion-resistant elements Zn and Ni accounts for more than 60% of the total nitrogen content, there is an excellent improvement in cell performance. However, excessive nitrogen content can lead to increased current collector impedance, affecting electron transport; while insufficient nitrogen content results in limited current collector ductility and corrosion resistance. Therefore, the elements in the positive electrode current collector are strongly correlated with the first solvent A and additive B. The differences are manifested in two ways: First, the number of exposed highly active corrosion sites varies, resulting in different required reaction equivalences for the first solvent A and additive B. Second, the differences in their ductility lead to spatially distributed stress in the active material, causing membrane rupture and repair, which also results in different required reaction equivalences for the first solvent A and additive B. By correlating and limiting the relationship between key components in the electrolyte and the nitrogen content of the positive electrode membrane current collector, the appropriate ratio and dosage of the first solvent A and additive B, while ensuring sufficient electron transport and minimal defects in the current collector, can prevent continuous oxidation of the electrolyte itself under high voltage, thus reducing power consumption (PF). 6- The decomposition rate avoids localized concentration of F at defect sites. - The rapid accumulation of HF species reduces the formation of microcracks and Al dissolution pits in the later stages of cycling, ensuring the adhesion between the material and the current collector, and effectively improving the cycling performance of high-voltage silicon-carbon systems. Detailed Implementation

[0032] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0033] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0034] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0035] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0036] Unless otherwise specified, all components, raw materials, or instruments used in the embodiments and comparative examples of this invention are commercially available, and the same type of components and raw materials are used in each parallel experiment.

[0037] In the first aspect of this application, the technical solution adopted by this application is: a secondary battery, including a positive electrode, a negative electrode, a separator and an electrolyte;

[0038] The positive electrode current collector contains nitrogen element, which includes at least one of Zn, Ni, Cr, Ca, and Ti.

[0039] The electrolyte comprises an organic solvent, a lithium salt, and an additive. The organic solvent comprises a first solvent and a second solvent. The first solvent is a halocarboxylic acid ester, which is a compound represented by structural formula A. The second solvent is at least one of a carbonate compound, a non-halocarboxylic acid ester compound, an ether compound, and a nitrile compound. The additive comprises a compound represented by structural formula B.

[0040]

[0041] In Formula A, R1 and R2 are each independently selected from one of halogen atoms, C1-C10 alkyl groups, and C1-C10 haloalkyl groups; and Formula A contains at least one halogen atom.

[0042] In formula B, R3, R4, R5, R6, and R7 are each independently selected from H atoms, halogen atoms, alkyl or olefinic groups with ≤3 carbon atoms, or halogenated or non-halogenated groups. One or more of the following; and formula B contains at least one halogen atom;

[0043] The secondary battery satisfies the following relationships: 1≤(X+50) / (P+10*Q)≤25, and 25≤X≤500, 3≤P≤50, 0.01≤Q≤5;

[0044] Where P is the weight percentage of the compound represented by structural formula A in the electrolyte;

[0045] Q represents the weight percentage of the compound represented by structural formula B in the electrolyte.

[0046] X represents the nitrogen content in the positive electrode current collector, expressed in ppm.

[0047] In some embodiments, the halogen atom is at least one of fluorine, chlorine, bromine, and iodine.

[0048] In some embodiments, structural formula A comprises at least one of the following compounds:

[0049]

[0050] The inventors of this application have discovered that after halogenation of compound A, the number of H substituents decreases, the molecular boiling point increases, and the self-thermal decomposition of the electrolyte at high temperatures is reduced. Furthermore, compound A has a lower HOMO value, which can improve the oxidation resistance of the electrolyte bulk, reduce the decomposition of solvent and lithium salt on the positive electrode side, and reduce the accumulation of byproducts at current collector defects.

[0051] In some embodiments, structural formula B comprises at least one of the following compounds:

[0052]

[0053] The inventors of this application have discovered that compound B has a high HOMO, and halogenation can reduce the electron cloud density of the pyridinium group in the molecular structure, lower the desolvation energy barrier, preferentially form a protective film on the cathode material over the solvent, regulate the dehydrogenation process of the carbonate solvent, reduce the local concentration of F- or HF species in the current collector, and reduce the corrosion effect on the current collector.

[0054] As an embodiment of this application, the secondary battery satisfies the following relationship: 5≤(X+50) / (P+10*Q)≤25, and 50≤X≤200, 5≤P≤30, 0.1≤Q≤2.

[0055] As an embodiment of this application, the positive current collector further contains aluminum; after the secondary battery is discharged, the aluminum content in the electrolyte is E, in ppm, which satisfies 80≤E≤210.

[0056] As an embodiment of this application, the N element contains Zn and / or Ni, and the mass percentage of the Zn and / or Ni elements, based on the total N element content, is F, which satisfies F≥60%.

[0057] As an embodiment of this application, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiDFP), lithium difluorobis(oxalate) phosphate (LiODFP), lithium tetrafluorooxalate phosphate (LiOTFP), lithium bis(oxalate) borate (LiBOB), lithium difluorobis(oxalate) borate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium 4,5-dicyano-2-(trifluoromethyl)isoimidazolium (LiTDI).

[0058] As an embodiment of this application, the additive further includes at least one of the following: 1,3-propanesulfonate lactone (PS), lithium difluorophosphate (LiDFP), lithium difluorobis(oxalate) phosphate (LiODFP), lithium tetrafluorooxalate phosphate (LiOTFP), lithium bis(oxalate) borate (LiBOB), lithium difluorobis(oxalate) borate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium 4,5-dicyano-2-(trifluoromethyl)isoimidazolium (LiTDI), sulfate ester compounds, and nitrile compounds.

[0059] As an embodiment of this application, the nitrile compounds include at least one selected from succinic anionyl nitrile, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexanetrionitrile, glyceryltrionitrile, adiponitrile, heptanonitrile, octanotrionitrile, anonadionitrile, and sebacate. The sulfate ester compounds include at least one selected from vinyl sulfate and fluorovinyl sulfate.

[0060] In some embodiments, the carbonate compound of the second solvent includes at least one selected from ethylene carbonate, fluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, vinylene carbonate, fluoroethyleneene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, and diphenyl carbonate; the non-halogenated carboxylic acid ester compound of the second solvent includes methyl formate, ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, and methyl propionate. The second solvent comprises at least one of ethyl butyrate, propyl butyrate, butyl butyrate, methyl butyrate, ethyl butyrate, propyl butyrate, and butyl butyrate; the ether compound of the second solvent comprises at least one of ethylene glycol dimethyl ether, 1,3-dioxolane, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether; the nitrile compound of the second solvent comprises at least one of succinic anionyl, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexanetrionitrile, glycerol trionitrile, adiponitrile, heptanonitrile, octanilide, nonadionitrile, and sebaconitrile.

[0061] In some embodiments, the lithium salt content is 8-25% by mass, the additive content is 0.01-15% by mass, and the second solvent content is 10-85% by mass, based on the mass percentage of the electrolyte.

[0062] For example, in the positive electrode sheet, the content X of element N is 25, 28, 30, 35, 38, 40, 45, 48, 50, 55, 58, 60, 65, 68, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 190, 200, 220, 250, 280, 300, 320, 350, 380, 400, 420, 450, 480, 500 or any two of these values.

[0063] For example, in the electrolyte, the weight percentage P of the compound with the structure shown in structural formula A is 3, 5, 8, 10, 15, 18, 20, 25, 28, 30, 35, 38, 40, 45, 48, 50 or any two of these values.

[0064] For example, in the electrolyte, the weight percentage Q of the compound with the structure shown in formula B is 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.2, 1.4, 1.5, 1.8, 2, 2.2, 2.4, 2.5, 2.8, 3, 3.2, 3.4, 3.5, 3.8, 4, 4.2, 4.4, 4.5, 4.8, 5, or a range of any two values ​​therein.

[0065] Solvent A has a lower HOMO value, which improves the oxidation resistance of the electrolyte bulk, reduces the decomposition of solvent and lithium salt on the positive electrode side, and further reduces the accumulation of by-products at current collector defects. Additive B has a higher HOMO value, and after halogenation, it can reduce the electron cloud density of the pyridine group in the molecular structure, lower the desolvation energy barrier, preferentially form a protective film on the positive electrode material compared to the solvent, regulate the dehydrogenation process of the carbonate solvent, and reduce the localized concentration of F in the current collector. - The presence of HF species can reduce the corrosion effect on the current collector. In the positive electrode current collector, the choice of different elements has varying degrees of improvement on the corrosion resistance and ductility of the current collector. Specifically, corrosion-resistant elements include Zn, Ni, and Cr. Zn can form a protective layer or metallic phase, improving corrosion resistance; Ni, as a stabilizer, is beneficial for forming high-melting-point intergranular compounds, inhibiting pitting corrosion; Cr is beneficial for forming an oxide film to inhibit corrosion. Furthermore, ductility-enhancing elements include Ca and Ti, both of which can refine grains and improve mechanical ductility. Extensive experimental data from researchers have shown that when nitrogen (N) contains both corrosion-resistant and ductility-enhancing elements, and when the total amount of corrosion-resistant elements Zn and Ni accounts for more than 60% of the total N content, there is an excellent improvement in cell performance. However, excessive N content can lead to increased current collector impedance, affecting electron transport; conversely, insufficient N content results in limited current collector ductility and corrosion resistance. Therefore, the elements in the positive electrode current collector are strongly correlated with the first solvent A and additive B. The differences are manifested in two ways: First, the number of exposed highly active corrosion sites varies, resulting in different required reaction equivalences for the first solvent A and additive B. Second, the differences in ductility lead to spatial stress distribution in the active material, causing membrane rupture and repair, which also results in different required reaction equivalences for the first solvent A and additive B. Excessive total nitrogen content increases current collector impedance, affecting electron transport; conversely, low total nitrogen content limits current collector ductility and corrosion resistance. By correlating and defining the relationship between key components in the electrolyte and the nitrogen content of the positive electrode membrane current collector, the appropriate ratio and dosage of the first solvent A and additive B, while ensuring sufficient electron transport and minimal defects in the current collector, can prevent continuous oxidation of the electrolyte itself under high voltage, thus reducing PF6. - The decomposition rate avoids localized concentration of F at defect sites. - The rapid accumulation of HF species reduces the formation of microcracks and Al dissolution pits in the later stages of cycling, ensuring the adhesion between the material and the current collector and improving the capacity stability of the cycle.

[0066] In some embodiments, the positive electrode sheet includes an aluminum foil current collector and a positive electrode membrane. The positive electrode membrane includes the positive electrode active material lithium cobalt oxide (LiCoO2), a conductive agent, and a binder. The conductive agent includes one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, and carbon nanofibers. The binder includes one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0067] The negative electrode includes a copper foil current collector and a negative electrode film. The negative electrode film includes the negative electrode active material graphite and the silicon-oxygen active material SiOx (or silicon-carbon active material SiC), a conductive agent, the thickener sodium carboxymethyl cellulose (CMC), and the binder polyacrylic acid PAA. The conductive agent includes one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, and carbon nanofibers.

[0068] In the secondary battery described in this invention, due to the applicability of the electrolyte, the active materials on the positive and negative electrodes can be selected from different types and combined as needed, all of which can achieve good electrochemical activity and safety stability.

[0069] A third aspect of this application provides an electrical device including the aforementioned secondary battery.

[0070] In specific embodiments of the present invention, the organic solvents and additives can be commercially purchased or self-made. Specifically, the preparation methods are all conventional synthesis methods, which will not be listed one by one here.

[0071] In a specific embodiment of this invention, the positive electrode current collector is deposited on the surface of aluminum foil using an electrochemical deposition method, ultimately obtaining thin films with different characteristic elements. This invention procures the corresponding current collector from a manufacturer capable of customizing aluminum foil modification; the current collector was purchased from Henan Mingtai Aluminum Industry.

[0072] Example 1

[0073] Electrolyte preparation: In an argon-filled glove box, EC, PC, PP, and first solvent A were first mixed in a mass ratio of 8:10:70.2:11.8 to obtain a mixed solution. Next, lithium salt LiPF6 (13% by weight of the total electrolyte), fluoroethylene carbonate (FEC) (12% by weight of the second solvent), 1,3-propanesulfonate lactone (PS) (2% by weight of the additive), 1,3,6-hexanetrionitrile (HTCN) (2% by weight of the additive), and additive B (3% by weight of the additive) were slowly added sequentially to the mixed solution. Finally, the mixture was stirred until homogeneous to obtain the electrolyte of Example 1, i.e., first solvent A accounted for 8% of the total electrolyte weight and additive B accounted for 3% of the total electrolyte weight.

[0074] Preparation of secondary batteries:

[0075] 1. Preparation of the positive electrode film: This includes the positive electrode active material lithium cobalt oxide (LiCoO2), the conductive agent Super P, and the binder polyvinylidene fluoride (PVDF). The materials are mixed in a weight ratio of LiCoO2:Super P:PVDF = 98.5:0.5:1, then added to N-methylpyrrolidone (NMP) and mixed thoroughly to prepare the positive electrode slurry for the lithium-ion battery cell. The positive electrode slurry is coated onto a current collector aluminum foil, dried at 85°C, cold-pressed, then trimmed and slit, dried under vacuum at 85°C for 4 hours, and finally the tabs are welded to prepare the positive electrode sheet.

[0076] 2. Preparation of the negative electrode film: This includes graphite and silicon carbide materials as negative electrode active materials, carbon nanotubes (CNTs) as conductive agents, sodium carboxymethyl cellulose (CMC) as a thickener, and polyacrylic acid (PAA) as a binder. The median particle size of the SiOx material is u = 4.8 μm. A mixture of graphite and silicon carbide materials at a weight ratio of 85:15 is used as the negative electrode active material. The negative electrode active material:CNT:CMC:PAA is mixed at a weight ratio of 97:0.8:1.2:1, and deionized water is added and mixed evenly to prepare the negative electrode slurry. The negative electrode slurry is coated on a copper foil current collector, dried at 85°C, cold-pressed, trimmed, and slit. After drying under vacuum at 85°C for 12 hours, tabs are welded to obtain the negative electrode sheet.

[0077] 3. Preparation of Soft-Pack Cells: The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in sequence, with the separator positioned between the positive and negative electrode sheets, and wound to obtain a bare cell. The cell is designed to have a capacity of 6.0 Ah and a voltage range of 3.0-4.55V. The bare cell is placed in an aluminum-plastic film outer packaging for sealing, and then baked in an 85℃ vacuum oven for 48 hours. Electrolyte is injected into the dried cell, followed by sealing, settling, formation, shaping, and capacity testing. A second sealing is then performed, achieving a electrolyte retention coefficient of 1.1 g / Ah, thus completing the preparation of the lithium-ion rechargeable soft-pack battery.

[0078] Comparative Examples 1-12 and Examples 2-29 illustrate the lithium-ion battery disclosed in this invention, including most of the operational steps in Example 1, such as electrolyte preparation: 100% of the total weight is reduced by 13% LiPF6, additives: 2% PS, 2% HTCN, second solvent: 12% FEC, and a specific amount of additive B, to obtain the remaining weight M. The percentage of the remaining weight M of the first solvent A is calculated based on its proportion to the total electrolyte weight. For example, in Example 16, the content of A is 3%, and the content of B is 5%, then M = 100% - 13% LiPF6 - 2% PS - 2% HTCN - 12% FEC - 5% additive B = 66%. Since A accounts for 3% of the total electrolyte content, A accounts for 4.5% of M, that is, the solvents in M ​​are EC:PC:PP:first solvent A = 8:10:77.5:4.5. In this invention, the proportions of EC and PC in the remaining weight M are fixed at 8% and 10%, respectively; while the proportion of PP in M ​​is M-8%EC-10%PC-first solvent A. The content variations of PP in the same amounts as other substances besides first solvent A and additive B are not listed or elaborated in Tables 1 and 2.

[0079] Other differences include: the types and contents of the first solvent, halocarboxylic acid ester A, and the key additive B are different; the types and contents of the key characteristic element N in the positive electrode current collector are also different. Specific values ​​are shown in Tables 1 and 2. Here, " / " indicates that the substance is not present. In the column for the types and contents of the characteristic element N in the positive electrode current collector, the types and contents are in a one-to-one correspondence. For example, in Example 16, the types are: Zn+Ni+Ca, and the contents are: 100+50+50=200, that is, Zn content 100, Ni content 50, Ca content 50, and total content 200. Other examples are not detailed here.

[0080] The following performance tests were performed on each secondary pouch cell:

[0081] (1) 45℃ High Temperature Cycling Test: In a 45℃ environment, the battery after capacity determination is charged to 4.55V at a constant current and constant voltage of 0.7C, with a cutoff current of 0.05C, and then discharged to 3.0V at a constant current of 0.5C. This cycle is repeated for 400 charge-discharge cycles. The capacity retention rate at the 400th cycle is calculated using the following formula:

[0082] 400-week cycle capacity retention (%) = (400-week cycle discharge capacity / initial cycle discharge capacity) × 100%;

[0083] The growth rate of the thickness in the 400th cycle (%) = (the full-charge thickness in the 400th week / the full-charge thickness in the first cycle) × 100%.

[0084] (2) Al content test in electrolyte: The lithium-ion battery was discharged and centrifuged in an environment of 25°C. The liquid obtained after centrifugation was subjected to inductively coupled plasma (ICP) for elemental monitoring to obtain the weight percentage of Al metal ions in the electrolyte.

[0085] (3) Determination of corrosion degree on the surface of the positive electrode current collector: After discharging the lithium-ion battery in an environment of 25℃, the battery was disassembled, and the aluminum current collector and electrode sheet in the exposed tab area of ​​the positive electrode film were taken. The exposed current collector area can be obtained by carefully wiping the electrode sheet with NMP. The exposed tab area and the exposed center area of ​​the electrode sheet that meet the above requirements were observed in a scanning electron microscope (SEM). At a magnification of 100, ≤10 corrosion holes in the image are defined as slight corrosion, 10 < ≤50 corrosion holes are defined as moderate corrosion, and 50 < ≤50 corrosion holes are defined as severe corrosion.

[0086] The test results are shown in Table 3.

[0087] Table 1

[0088]

[0089]

[0090] Table 2

[0091]

[0092] Table 3

[0093]

[0094] Comparing the results in Tables 1 and 2, and based on Examples 1-29 and Comparative Examples 1-12, it can be seen that when the weight percentages of compounds with the structure shown in structural formula A (first solvent) in different types of electrolytes, the weight percentages of compounds with the structure shown in structural formula B (key additive) in different types of electrolytes, and the content of the characteristic element N in different types of positive electrode current collectors satisfy the formula 1≤(X+50) / (P+10*Q)≤25, and 25≤X≤500, 3≤P≤50, and 0.01≤Q≤5, the obtained battery positive electrode current collector corrosion rate is [data missing]. The low degree of corrosion, low aluminum ion dissolution, high high-temperature cycling capacity retention, and low expansion rate indicate that the first solvent A participates in the solvation process and affects the internal and external arrangement of the key additive B in the solvated sheath, thereby affecting its electrochemical oxidation film formation effect. Furthermore, the key characteristic elements affect the electron transport and defect degree of the current collector. The synergistic film formation effect of the first solvent A and the additive B minimizes the continuous oxidation of the electrolyte on the positive electrode side, reduces the decomposition rate of PF6-, and avoids the rapid accumulation of F- or HF species locally concentrated at defect sites.

[0095] As shown in Examples 1-27, when different types of first solvent A, different types of key additive B, and different types of positive electrode film current collector characteristic element X further satisfy the formula 5≤(X+50) / (P+10*Q)≤25, and 50≤X≤200, 5≤P≤30, 0.1≤Q≤2, the lithium-ion battery exhibits lower corrosion of the positive electrode current collector and better high-temperature cycle performance. This indicates that the first solvent A, key additive B, and positive electrode film current collector characteristic element X are within the preferred range of this application and satisfy the formula 5≤(X+50) / (P+10*Q)≤25, thus exhibiting stronger correlation characteristics among the three, resulting in better cell performance.

[0096] As demonstrated in Examples 27-29, the performance of the battery cell was further improved by introducing additional additives, such as succinate (SN) and vinylene carbonate (VC), into the electrolyte. It is speculated that these additives synergistically participate in the formation of the electrode interface film, reducing the local enrichment of F- and HF, and preventing the corrosion reaction from proceeding too rapidly.

[0097] As can be seen from Comparative Examples 8-10, even if the first solvent A, the key additive B, and the characteristic element X of the positive electrode membrane current collector in different types of electrolytes satisfy the formula 1≤(X+50) / (P+10*Q)≤25, the contents of A, B, and X do not meet the range limit, and the cell does not have excellent performance.

[0098] Comparative Examples 11 and 12 show that even if the first solvent A in different types of electrolytes, the key additives B in different types of electrolytes, and the characteristic elements of the positive electrode membrane current collector in different types of electrolytes meet their respective range limits, the cell performance is still lacking if the formula 1≤(X+50) / (P+10*Q)≤25 is not satisfied. This demonstrates a strong correlation between parameters A, B, and X. Formula 1≤(X+50) / (P+10*Q)≤25 can comprehensively correlate various influencing factors, achieving a better synergistic effect.

[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A secondary battery characterized by comprising: Includes positive electrode, negative electrode, separator and electrolyte; The positive electrode current collector contains nitrogen element, including Zn, Ni, Cr, Ca, and Ti; The electrolyte comprises an organic solvent, a lithium salt, and an additive. The organic solvent comprises a first solvent and a second solvent. The first solvent is a halocarboxylic acid ester, which is a compound with structural formula A. The second solvent is at least one of a carbonate compound, a non-halocarboxylic acid ester compound, an ether compound, and a nitrile compound. The additive includes the compound shown in structural formula B; AB; In Formula A, R1 and R2 are each independently selected from one of halogen atoms, C1-C10 alkyl groups, and C1-C10 haloalkyl groups; and Formula A contains at least one halogen atom. In formula B, R3, R4, R5, R6, and R7 are each independently selected from the number of H atoms, halogen atoms, and carbon atoms. ≤3 halogenated or non-halogenated alkyl or olefinic groups, , One or more of the following; and formula B contains at least one halogen atom; The secondary battery satisfies the following relationships: 1≤(X+50) / (P+10*Q)≤25, and 25≤X≤500, 3≤P≤50, 0.01≤Q≤5; Where P is the weight percentage of the compound represented by structural formula A in the electrolyte; Q represents the weight percentage of the compound represented by structural formula B in the electrolyte. X represents the nitrogen content in the positive electrode current collector, expressed in ppm.

2. The secondary battery as described in claim 1, characterized in that, The structural formula A includes at least one of the following compounds:

3. The secondary battery as described in claim 1, characterized in that, The structural formula B includes at least one of the following compounds:

4. The secondary battery as described in claim 1, characterized in that, The positive electrode current collector also contains aluminum; after the secondary battery is discharged, the aluminum content in the electrolyte is E, in ppm, which satisfies 80≤E≤210.

5. The secondary battery as described in claim 1, characterized in that, The N element contains Zn and Ni, and the mass percentage of Zn and Ni elements, based on the total N element content, is F, which satisfies F≥60%.

6. The secondary battery as described in claim 1, characterized in that, The lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, lithium tetrafluorooxalate phosphate, lithium bis(oxalate) borate, lithium difluorooxalate borate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium 4,5-dicyano-2-(trifluoromethyl)isoimidazole.

7. The secondary battery as described in claim 1, characterized in that, The additives also include at least one of the following: 1,3-propanesulfonate lactone, lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, lithium tetrafluorooxalate phosphate, lithium bis(oxalate) borate, lithium difluorobis(oxalate) borate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium 4,5-dicyano-2-(trifluoromethyl)isoimidazole, nitrile compounds, and sulfate compounds.

8. The secondary battery as described in claim 1, characterized in that, The carbonate compound of the second solvent includes at least one selected from ethylene carbonate, fluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, vinylene carbonate, fluoroethyleneene carbonate, dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, and diphenyl carbonate; the non-halogenated carboxylic acid ester compound of the second solvent includes at least one selected from methyl formate, ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, and butyl butyrate; the ether compound of the second solvent includes ethylene glycol dimethyl ether, 1,3-dioxolane, and 1,1,2,2-tetrafluoroethyl-2,2,3-dioxolane. At least one of 3-tetrafluoropropyl ether; the nitrile compound of the second solvent includes at least one of succinic acid, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexanetrionitrile, glycerol trionitrile, adiponitrile, heptanonitrile, octadionitrile, nonadionitrile, and sebaconitrile.

9. The secondary battery as described in claim 1, characterized in that, Based on the mass percentage of the electrolyte, the lithium salt has a mass percentage of 8-25%, the additive has a mass percentage of 0.01-15%, and the second solvent has a mass percentage of 10-85%.

10. The secondary battery as described in claim 1, characterized in that, The negative electrode sheet includes a negative electrode material, which includes at least one of lithium metal, graphite, silicon-oxygen composite material and silicon-carbon composite material.

11. An electrical appliance, characterized in that, Includes the secondary battery as described in any one of claims 1-8.

Citation Information

Patent Citations

  • Nonaqueous electrolytic solution and nonaqueous electrolytic solution secondary battery

    CN107666011A

  • Electrolytic solution, electrochemical device, lithium ion secondary battery, and module

    CN110495041A