Polypropylene hydrophilic modification method, obtained material and container cover made of material

Through the melt grafting method of introducing hydrophilic groups into polypropylene, the problem of water drops on the container lid is solved, the water film phenomenon and rapid volatility are achieved, and the user experience of the container lid is improved.

CN120329676APending Publication Date: 2025-07-18THERMOS CHINA HOUSEWARES

Patent Information

Application Number
CN202510645499.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-20
Publication Date
2025-07-18

AI Technical Summary

Technical Problem

The problem of existing container lids forming water droplets and spilling after high-temperature steam contact, resulting in inconvenience in use, the existing solution materials are wasted and the appearance is not beautiful.

Method used

The hydrophilic group is introduced into the polypropylene by melt grafting method, and a hydrophilic polypropylene composite material is prepared by mixing the polypropylene substrate, graft monomer, initiator, polyethylene glycol and antioxidant to improve its hydrophilicity and thermal stability.

Benefits of technology

It improves the phenomenon of water droplets falling into water film, improves the volatility of moisture, enhances the dryness of use, and improves the user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120329676A_ABST
    Figure CN120329676A_ABST
Patent Text Reader

Abstract

The invention relates to a polypropylene hydrophilic modification method, an obtained material and a container cover prepared from the material. The hydrophilic modification method of the polypropylene comprises the following steps: uniformly mixing the components of the raw materials; adding the mixture into a double-screw extruder for melt grafting; and cooling the polymer melt extruded by the twin-screw extruder with water to obtain solid polymer strips, drying the polymer strips, and granulating to obtain hydrophilic polypropylene particles, namely the hydrophilic polypropylene composite material. The high-performance hydrophilic polypropylene composite material disclosed by the invention has excellent mechanical properties, the hydrophilic performance is also greatly improved, and the preparation process is simple. According to the container cover made of the material, the problems that water drops adhere to the container cover due to water vapor condensation and water drops scatter when the container cover is opened can be solved, the water drop phenomenon is improved into the water film phenomenon, the water drops scatter when the container cover is opened is avoided, the volatilization speed of water on the surface of the container cover is increased, and therefore the use dryness is enhanced, and the use experience of a user is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for hydrophilic modification of polypropylene, the obtained material and a container lid made therefrom. By using the hydrophilic property of the modified material obtained by this method, the problem of water droplet adhesion caused by water vapor condensation during actual use of the container lid is improved, belonging to the fields of polymer material modification and container lids. Background Art

[0002] As a general-purpose plastic, polypropylene is widely used in container lid products for storing food and beverages due to its low price, good toughness and strength properties. However, when the container contains hot water, soup and other contents with higher temperature during actual use of such products, due to the phenomenon of water vapor condensation caused by the contact of high-temperature steam with the container lid, a large number of water droplets are formed at the lower end of the container lid, and the problem of water droplets spilling during opening of the lid will cause pollution to the tabletop and the ground, resulting in inconvenient use.

[0003] In order to improve the problem of water droplet spilling at the lower end of the container lid, represented by the invention patent with the patent number 202010423953.4 and the authorized publication number CN111977160B applied by the applicant's research team, the prior art usually needs to add ribs with a certain height at the lower end of the container lid or at the lower edge of the container lid sealing ring to collect water droplets. However, such structures cause disadvantages such as waste of production materials, unappealing appearance and inconvenient cleaning. Summary of the Invention

[0004] The main object of the present invention is to overcome the problems existing in the prior art, and provide a method for hydrophilic modification of polypropylene, the material obtained by this method and a container lid made of this material, which can improve the problems of water droplet adhesion and water droplet spilling during opening of the lid caused by water vapor condensation, change the water droplet phenomenon into a water film phenomenon, avoid water droplet spilling during opening of the lid, and improve the evaporation rate of the moisture on the surface of the container lid.

[0005] The technical solution for the present invention to solve its technical problems is as follows: A method for hydrophilic modification of polypropylene, comprising the following steps: First step, mixing polypropylene substrate, graft monomer, initiator, polyethylene glycol, antioxidant to make each component uniformly dispersed; wherein, the graft monomer adopts p-allylstyrene and ethylene-vinyl acetate copolymer, and the initiator adopts diisopropylbenzene peroxide; the weight percentages of each component are as follows: Polypropylene substrate 77.2 - 91.55%, Polyethylene glycol 5.0 - 10.0%, Ethylene-vinyl acetate copolymer 3.0 - 10.0%, p-allylstyrene 0.3 - 2.0%, Initiator 0.05 - 0.3%, Antioxidant: 0.1 - 0.5%; Step 2: Add the mixed materials into a twin - screw extruder for melt grafting; Step 3: Cool the polymer melt extruded from the twin - screw extruder with water to obtain a solid polymer strip. After drying the polymer strip, pelletize it to obtain hydrophilic polypropylene particles, which are the hydrophilic polypropylene composite material.

[0006] This method uses the melt grafting method to graft hydrophilic groups onto ordinary polypropylene to make hydrophilic polypropylene, enabling the originally hydrophobic polypropylene surface to form hydrogen bonds with water molecules and having higher thermal stability. After this modification treatment, the obtained hydrophilic polypropylene composite material has a significantly lower water contact angle than ordinary polypropylene, thus having better hydrophilicity. When a container lid made of this material comes into contact with water vapor, since water spreads on its surface to form a water film, the evaporation efficiency increases after standing, so it dries faster.

[0007] The further improved technical solution of the present invention is as follows: Preferably, in the first step, the polypropylene substrate uses homopolypropylene, the number - average molecular weight of polyethylene glycol > 4000; the antioxidant uses a compound antioxidant composed of a primary antioxidant and a secondary antioxidant, where the primary antioxidant is antioxidant 1010 or antioxidant 3114, and the secondary antioxidant is antioxidant 168 or antioxidant 618.

[0008] Preferably, in the first step, the mixing is carried out in a high - speed mixer, the mixing time is 2 - 15 minutes, and the stirring speed is 800 - 1200 r / min.

[0009] Adopting the above - mentioned preferred scheme can further optimize the specific technical details of the first step.

[0010] Preferably, in the second step, the temperature of the twin - screw extruder is set at 190°C - 230°C, the screw speed is 200 - 400 r / min, and the residence time of the material in the twin - screw extruder is 40 - 75 seconds.

[0011] Adopting the above - mentioned preferred scheme can further optimize the specific technical details of the second step.

[0012] Preferably, in the third step, circulating water is used for cooling; the drying method is air drying.

[0013] Preferably, the third step further includes: screening and packaging the hydrophilic polypropylene particles for later use.

[0014] Adopting the above - mentioned preferred scheme can further optimize the specific technical details of the third step.

[0015] The present invention also provides: A high-performance hydrophilic polypropylene composite material prepared by the polypropylene hydrophilic modification method described above.

[0016] The present invention also provides: A container lid made from a raw material containing the high-performance hydrophilic polypropylene composite material described above.

[0017] Preferably, the raw material consists of polypropylene and the high-performance hydrophilic polypropylene composite material.

[0018] Preferably, the weight percentage of the high-performance hydrophilic polypropylene composite material in the total amount of the raw material is ≥5%.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: The high-performance hydrophilic polypropylene composite material of the present invention has excellent mechanical properties, and at the same time, the hydrophilic property is also greatly improved, and the preparation process is simple. The container lid (such as cup lid, pot lid, lunch box lid, etc.) made of this material can improve the problems of water droplet adhesion caused by water vapor condensation on the container lid and water droplet spillage when opening the lid, change the water droplet phenomenon into a water film phenomenon, avoid water droplet spillage when opening the lid, and increase the evaporation rate of the moisture on the surface of the container lid, thereby enhancing the dryness during use and improving the user experience. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is the main principle of the polypropylene hydrophilic modification method of the present invention.

[0021] Figure 2 It is the production process flow chart of Example 1 of the present invention.

[0022] Figure 3 It is the test result of the control group of Test 1 in Example 2 of the present invention.

[0023] Figure 4 It is the test result of the sample group of Test 1 in Example 2 of the present invention.

[0024] Figure 5 It is the test result of the control group of Test 2 in Example 2 of the present invention.

[0025] Figure 6 It is the test result of the sample group of Test 2 in Example 2 of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0026] The main research idea of the present invention is as follows: Ordinary polypropylene is originally a hydrophobic material that cannot form hydrogen bonds with water molecules. When it encounters water vapor and cools down, water droplets will form on its surface. The inventor's research team once tried to add hydrophilic or polar polymers to polypropylene, such as polypropylene grafted acrylic acid copolymer and ethylene acrylic acid copolymer, to improve hydrophilicity by blending modification. However, although this method can reduce the water contact angle, its stability is poor, especially when it encounters hot water vapor, it has no effect.

[0027] After practical research, the inventor's research team adopted the method of melt grafting to graft hydrophilic groups onto ordinary polypropylene to make hydrophilic polypropylene, enabling the originally hydrophobic polypropylene surface to form hydrogen bonds with water molecules and having higher thermal stability. After this modification treatment, the water contact angle of the obtained hydrophilic polypropylene composite material is significantly lower than that of ordinary polypropylene, thus having better hydrophilicity. When the container lid made of this material comes into contact with water vapor, water spreads out on the surface, the evaporation efficiency increases after placement, and it will dry faster.

[0028] Specifically in implementation, the polypropylene hydrophilic modification method of the present invention includes the following steps: First step, mix polypropylene substrate, graft monomer, initiator, polyethylene glycol, and antioxidant to make each component evenly dispersed; among them, the graft monomer adopts p-allylstyrene and ethylene-vinyl acetate copolymer (i.e., EVA), and the initiator adopts dicumyl peroxide (i.e., DCP); the weight percentages of each component are as follows: Polypropylene substrate 77.2 - 91.55%, Polyethylene glycol 5.0 - 10.0%, Ethylene-vinyl acetate copolymer 3.0 - 10.0%, p-allylstyrene 0.3 - 2.0%, Initiator 0.05 - 0.3%, Antioxidant 0.1 - 0.5%; In addition, the polypropylene substrate adopts homopolypropylene, and the number average molecular weight of polyethylene glycol > 4000; the antioxidant adopts a compound antioxidant composed of a main antioxidant and an auxiliary antioxidant, where the main antioxidant is antioxidant 1010 or antioxidant 3114, and the auxiliary antioxidant is antioxidant 168 or antioxidant 618 (for example, a compound antioxidant composed of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:2); the mixing is carried out in a high-speed mixer, the mixing time is 2 - 15 minutes, and the stirring speed is 800 - 1200 r / min.

[0029] Step 2: Add the mixed materials into a twin-screw extruder for melt grafting. The twin-screw extruder adopted has great shear force and self-cleaning ability, which can increase the specific surface area of the polypropylene melt, facilitate mass transfer, enable the polypropylene and the grafting monomer to be quickly and fully mixed, and ensure the grafting rate and the uniformity of the grafting product.

[0030] Among them, the temperature of the twin-screw extruder is set at 190°C - 230°C (i.e., the polypropylene melt grafting is carried out above the melting point of polypropylene), the screw speed is 200 - 400 r / min, and the residence time of the materials in the twin-screw extruder is 40 - 75 seconds.

[0031] Step 3: Cool the polymer melt extruded from the twin-screw extruder with water to obtain a solid polymer strip. After drying the polymer strip, pelletize it to obtain hydrophilic polypropylene particles, which are the hydrophilic polypropylene composite material.

[0032] Among them, circulating water is used for cooling; the drying method is air drying. In addition, the hydrophilic polypropylene particles are sieved and packaged for standby.

[0033] The main principle of the above polypropylene hydrophilic modification method is as Figure 1 shown: Under the action of the DCP initiator, the polymer molecular chain breaks and degrades; hydrophilic groups are grafted; and continuous production is realized by reactive extrusion. Note: Figure 1 Among them, "high polymer" is ethylene-vinyl acetate copolymer; "acrylic monomer" comes from polypropylene; "free radical stabilizer" is antioxidant; "functional high polymer" is hydrophilic polypropylene.

[0034] The present invention will be further described in detail below with reference to the accompanying drawings and in combination with embodiments. However, the present invention is not limited to the given examples.

[0035] Example 1 In this example, a hydrophilic polypropylene composite material is obtained by hydrophilic modification of polypropylene.

[0036] The specific content of this example is as follows: 1. Raw material preparation (1) Polypropylene substrate: Homopolypropylene is adopted.

[0037] (2) Grafting monomer: p-allylstyrene and ethylene-vinyl acetate copolymer (i.e., EVA) are adopted.

[0038] (3) Initiator: Dicumyl peroxide (DCP) is adopted.

[0039] (4) Polyethylene glycol (number average molecular weight > 4000).

[0040] (5) Antioxidant: A compound antioxidant composed of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:2 is used.

[0041] The weight percentages of each component are as follows: Homopolypropylene 77.2 - 91.55%, Polyethylene glycol 5.0 - 10.0%, Ethylene - vinyl acetate copolymer 3.0 - 10.0%, p - allylstyrene 0.3 - 2.0%, DCP initiator 0.05 - 0.3%, Antioxidant 0.1 - 0.5%.

[0042] 2. Mixing Mix the polypropylene substrate, graft monomer, initiator, polyethylene glycol, and antioxidant in a high - speed mixer in a predetermined ratio to ensure uniform dispersion of each component. Among them, the mixing time is 2 - 15 minutes, and the stirring speed is 800 - 1200 r / min.

[0043] 3. Melt grafting reaction Add the mixed material into a twin - screw extruder for melt grafting. The temperature of the twin - screw extruder is set at 190°C - 230°C, the screw speed is 200 - 400 r / min, and the residence time of the material in the twin - screw extruder is 40 - 75 seconds.

[0044] 4. Extrusion and pelletizing Use circulating water to cool the polymer melt extruded from the twin - screw extruder into a solid polymer strip. After air - drying, cut the polymer strip to obtain hydrophilic polypropylene particles, which are the hydrophilic polypropylene composite material. Then, sieve and package for standby.

[0045] The production process flow chart of this embodiment is as Figure 2 shown, where 01 is a high - speed mixer, 02 is a twin - screw extruder, 03 is a cooling process, 04 is a pelletizing process, 05 is a sieving process, and 06 is a packaging process.

[0046] The examples of this embodiment and the blank comparative example for comparison are as follows: (1) Example 1 1 - 1. Raw material preparation The weight parts of each component are: Homopolypropylene 90.6 parts, polyethylene glycol (number - average molecular weight > 4000) 8 parts, ethylene - vinyl acetate copolymer 3.1 parts, p - allylstyrene 0.8 parts, DCP initiator 0.1 part, antioxidant 0.2 part.

[0047] 1 - 2. Mixing Mix the above components in a high-speed mixer to ensure uniform dispersion of each component. Among them, the mixing time is 10 minutes and the stirring speed is 800 - 1000 r / min.

[0048] 1 - 3. Melt grafting reaction Add the mixed material into a twin-screw extruder for melt grafting. The temperature of the twin-screw extruder is set at 190°C - 230°C, the screw speed is 300 - 400 r / min, and the residence time of the material in the twin-screw extruder is 55 - 65 seconds.

[0049] 1 - 4. Extrusion and pelletization Use circulating water to cool the polymer melt extruded from the twin-screw extruder into a solid polymer strip. After air drying, pelletize the polymer strip to obtain hydrophilic polypropylene particles.

[0050] (2) Example 2 2 - 1. Raw material preparation The weight parts of each component are as follows: 92.6 parts of homopolypropylene, 6 parts of polyethylene glycol (number average molecular weight > 4000), 5 parts of ethylene-vinyl acetate copolymer, 0.4 part of p-allylstyrene, 0.2 part of DCP initiator, 0.2 part of antioxidant.

[0051] 2 - 2. Mixing Mix the above components in a high-speed mixer to ensure uniform dispersion of each component. Among them, the mixing time is 8 minutes and the stirring speed is 1000 - 1200 r / min.

[0052] 2 - 3. Melt grafting reaction Add the mixed material into a twin-screw extruder for melt grafting. The temperature of the twin-screw extruder is set at 190°C - 220°C, the screw speed is 200 - 300 r / min, and the residence time of the material in the twin-screw extruder is 65 - 75 seconds.

[0053] 2 - 4. Extrusion and pelletization Use circulating water to cool the polymer melt extruded from the twin-screw extruder into a solid polymer strip. After air drying, pelletize the polymer strip to obtain hydrophilic polypropylene particles.

[0054] (3) Example 3 3 - 1. Raw material preparation The weight parts of each component are as follows: 92.6 parts of homopolypropylene, 10 parts of polyethylene glycol (number average molecular weight > 4000), 10 parts of ethylene-vinyl acetate copolymer, 1.8 parts of p-allylstyrene, 0.2 parts of DCP initiator, 0.2 parts of antioxidant.

[0055] 3-2. Mixing Mix the above components in a high-speed mixer to ensure uniform dispersion of each component. Among them, the mixing time is 15 minutes and the stirring speed is 1000 - 1200 r / min.

[0056] 3-3. Melt grafting reaction Add the mixed materials into a twin-screw extruder for melt grafting. The temperature of the twin-screw extruder is set at 190°C - 220°C, the screw speed is 300 - 400 r / min, and the residence time of the materials in the twin-screw extruder is 40 - 45 seconds.

[0057] 3-4. Extrusion and pelletizing Use circulating water to cool the polymer melt extruded from the twin-screw extruder into a solid polymer strip. After air drying, cut the polymer strip to obtain hydrophilic polypropylene particles.

[0058] (4) Blank control example 4-1. Raw material preparation The weight parts of each component are: 89.8 parts of homopolypropylene, 10 parts of ethylene-vinyl acetate copolymer, 0.2 parts of antioxidant.

[0059] 4-2. Mixing Mix the above components in a high-speed mixer to ensure uniform dispersion of each component. Among them, the mixing time is 10 minutes and the stirring speed is 800 - 1000 r / min.

[0060] 4-3. Melt grafting reaction Add the mixed materials into a twin-screw extruder for melt grafting. The temperature of the twin-screw extruder is set at 190°C - 230°C, the screw speed is 300 - 400 r / min, and the residence time of the materials in the twin-screw extruder is 55 - 65 seconds.

[0061] 4-4. Extrusion and pelletizing Use circulating water to cool the polymer melt extruded from the twin-screw extruder into a solid polymer strip. After air drying, cut the polymer strip to obtain polypropylene particles.

[0062] Take the materials obtained from the above examples and the blank control example as samples and conduct the following tests respectively: (1) Izod notched impact strength: The notched impact strength of each sample was measured using an impact testing machine (XJU-22, Chengde, China). Before testing, it was maintained at 20 °C for 12 hours. Five specimens (length × width × height = 80 × 10 × 4 mm 3 ) were tested for each sample to obtain an average notched depth of 2 mm.

[0063] (2) Tensile strength: The tensile properties of each sample were measured using an electronic universal testing machine in accordance with GB / T1040.1—2018 at a tensile speed of 50 m / min under the test conditions (temperature 23 °C, humidity 50%), and the average value was taken after five tests.

[0064] (3) Contact angle: It was measured by using profile image analysis: A pure water droplet was dropped on the surface of the solid sample, and the profile image of the droplet was obtained through a microscope lens and a camera. Then, the contact angle of the droplet in the image was calculated using existing digital image processing and algorithms.

[0065] The test results of each sample are shown in Table 1 below: Table 1

[0066] It can be seen from the above results that compared with the blank control example, each sample in this example has excellent mechanical properties and greatly improved hydrophilic properties; and due to the presence of ethylene-vinyl acetate copolymer, it plays a role in toughening polypropylene, making the toughness of the obtained material significantly improved.

[0067] At the same time, the preparation process of the present invention is simple, and the obtained hydrophilic polypropylene particles have characteristic polar functional groups, have diversity in post-processing, and have strong application prospects.

[0068] Example 2 In this example, a dew condensation test was carried out to verify the use effect of the hydrophilic polypropylene composite material of the present invention.

[0069] The specific content of this example is as follows: Raw materials: (1) Commercially available polypropylene material: PP 6331 produced by Lee Chang Yung Chemical Industry Co., Ltd.

[0070] (2) Hydrophilic polypropylene composite material: The hydrophilic polypropylene composite material was prepared according to Example 1, Example 1.

[0071] Test 1: The product JDG-450 of our company was used as the test water cup.

[0072] Control group: A cup cover matching the test water cup was made of commercially available polypropylene material.

[0073] Sample group: After adding 10% of hydrophilic polypropylene composite material by weight to commercially available polypropylene materials, cup lids matching the test water cups were made.

[0074] Test method: Fill the water cup with boiling water, cover the cup lid, and after placing it for 10 minutes, open the lid and check the dew condensation condition of the cup lid; place the cup lid upside down and flat for two minutes, and then check the surface condition of the cup lid. Three parallel tests were conducted for each group.

[0075] Test results: The test results of the three parallel tests of the control group are as Figure 3 shown. Water droplets formed on the surfaces of the cup lids when the lids were opened, and they were still not easily volatilized when placed upside down and flat. The test results of the three parallel tests of the sample group are as Figure 4 shown. A water film or water mark was locally formed on the surfaces of the cup lids when the lids were opened, and the volatilization rate was relatively fast when placed upside down and flat.

[0076] During the test, the weights of the cup lids were measured before the test, when the lids were opened (weighing immediately after removing the cup lids), and when placed upside down and flat for two minutes, respectively. The results are shown in Table 2 below.

[0077] Table 2

[0078] It can be seen from Table 2 that compared with the data of the control group, the weight gain of the cup lids in the sample group when the lids were opened was significantly lower, and the percentage of the water volume volatilized when placed upside down and flat for two minutes was significantly higher, that is, the volatilization efficiency was significantly higher.

[0079] Test two: The product GBM-021 of our company was used as the test water cup.

[0080] Control group: Cup lids matching the test water cups were made of commercially available polypropylene materials.

[0081] Sample group: After adding 10% of hydrophilic polypropylene composite material by weight to commercially available polypropylene materials, cup lids matching the test water cups were made.

[0082] Test method: Fill the water cup with boiling water, cover the cup lid, and after placing it for 10 minutes, open the lid and check the dew condensation condition of the cup lid; place the cup lid upside down and flat. During the test, the weights of the cup lids were measured before the test, when the lids were opened (weighing immediately after removing the cup lids), when placed upside down and flat for 30 seconds, and when placed upside down and flat for 60 seconds, respectively, and photos were taken. Five parallel tests were conducted for each group.

[0083] Test results: The test results of the control group are as Figure 5 shown. Water droplets formed on the surfaces of the cup lids when the lids were opened, and they were still not easily volatilized when placed upside down and flat. The test results of the sample group are as Figure 6As shown, when the lid is opened, a water film or watermark is locally formed on the surface of each cup lid, and the evaporation rate is relatively fast when it is placed upside down and flat.

[0084] The weighing results are shown in Table 3 below.

[0085] Table 3

[0086] It can be seen from Table 3 that: compared with the data of the control group, the weight gain of the cup lids in the sample group is significantly lower when the lid is opened, and the evaporation efficiency is significantly higher when it is placed upside down and flat.

[0087] Based on the above embodiments, the high-performance hydrophilic polypropylene composite material prepared by the present invention has excellent mechanical properties, and at the same time, the hydrophilic property is also greatly improved, and the preparation process is simple. The container lids (such as cup lids, pot lids, lunch box lids, etc.) made of this material can improve the problems of water droplet attachment caused by water vapor condensation and water droplet splashing when the lid is opened, change the water droplet phenomenon into a water film phenomenon, avoid water droplet splashing when the lid is opened, and improve the evaporation rate of the moisture on the surface of the container lid, thereby enhancing the dryness during use and improving the user experience.

[0088] In addition to the above embodiments, the present invention may have other embodiments. Any technical solutions formed by equivalent replacement or equivalent transformation fall within the protection scope required by the present invention.

Claims

1. A method for hydrophilic modification of polypropylene, characterized in that, It includes the following steps: First step: Mix the polypropylene substrate, graft monomer, initiator, polyethylene glycol, and antioxidant to uniformly disperse each component; wherein, the graft monomer uses p-allylstyrene and ethylene-vinyl acetate copolymer, and the initiator uses dicumyl peroxide; the weight percentages of each component are as follows: Polypropylene substrate 77.2 - 91.55%, Polyethylene glycol 5.0 - 10.0%, Ethylene-vinyl acetate copolymer 3.0 - 10.0%, p-allylstyrene 0.3 - 2.0%, Initiator 0.05 - 0.3%, Antioxidant 0.1 - 0.5%; Second step: Add the mixed material into a twin-screw extruder for melt grafting; Third step: Cool the polymer melt extruded from the twin-screw extruder with water to obtain a solid polymer strip, dry the polymer strip and then pelletize it to obtain hydrophilic polypropylene particles, which are the hydrophilic polypropylene composite material.

2. A method for hydrophilic modification of polypropylene according to claim 1, wherein in the first step, the polypropylene substrate uses homopolypropylene, and the number-average molecular weight of the polyethylene glycol > 4000; the antioxidant uses a compound antioxidant composed of a primary antioxidant and a secondary antioxidant, wherein the primary antioxidant is antioxidant 1010 or antioxidant 3114, and the secondary antioxidant is antioxidant 168 or antioxidant 618.

3. A method for hydrophilic modification of polypropylene according to claim 1, wherein in the first step, the mixing is carried out in a high-speed mixer, the mixing time is 2 - 15 minutes, and the stirring speed is 800 - 1200 r / min.

4. A method for hydrophilic modification of polypropylene according to claim 1, wherein in the second step, the temperature of the twin-screw extruder is set at 190°C - 230°C, the screw speed is 200 - 400 r / min, and the residence time of the material in the twin-screw extruder is 40 - 75 seconds.

5. A method for hydrophilic modification of polypropylene according to any one of claims 1 to 4, characterized in that, In the third step, circulating water is used for cooling; the drying method is air drying.

6. A polypropylene hydrophilic modification method according to any one of claims 1 to 4, characterized in that, The third step further includes: Screening and packaging the hydrophilic polypropylene particles for standby.

7. A high-performance hydrophilic polypropylene composite material prepared by the method for hydrophilic modification of polypropylene according to any one of claims 1 to 6.

8. A container lid, characterized in that, Prepared from raw materials containing the high-performance hydrophilic polypropylene composite material described in claim 7.

9. The container lid according to claim 8, characterized in that, The raw materials are composed of polypropylene and the high-performance hydrophilic polypropylene composite material.

10. A container lid according to claim 8, characterized in that, The weight percentage of the high-performance hydrophilic polypropylene composite material in the total amount of raw materials ≥ 5%.

Citation Information

Patent Citations

  • Cover unit and covered container

    CN111977160B

Cited By

  • Preparation method of hydrophilic polypropylene material

    CN121779820A