Non-aqueous electrolyte and sodium-ion battery containing the non-aqueous electrolyte
By using compounds A and B to form a uniform and dense SEI film in sodium-ion batteries, the problem of SEI film instability was solved, and the high-temperature storage and low-temperature cycling performance of the battery was improved.
Patent Information
- Application Number
- CN202510547132.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-04-28
AI Technical Summary
Sodium-ion batteries suffer from uneven and poorly dense solid electrolyte interphase (SEI) films, resulting in insufficient thermodynamic stability and poor high-temperature storage and low-temperature cycling performance.
Compounds A and B from the non-aqueous electrolyte are used as additives to form a uniform, dense, and thermodynamically stable SEI film, which is rich in inorganic sodium salts and works synergistically to improve the stability of the SEI film.
It significantly improves the high-temperature storage performance and high- and low-temperature cycling performance of sodium-ion batteries, and enhances the protective effect of electrode materials.
Smart Images

Figure CN120376752B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of secondary battery technology, and particularly relates to a non-aqueous electrolyte and a sodium-ion battery containing the non-aqueous electrolyte. Background Technology
[0002] Rechargeable sodium-ion batteries (SIBs) have broad application prospects in large-scale energy storage due to the abundance and low cost of sodium resources, and are particularly suitable for addressing the needs of global energy demand growth and sustainable development. Furthermore, their structure and working principle are similar to mature lithium-ion batteries, allowing for accelerated commercialization through existing production technologies. However, sodium-ion batteries still face key challenges, with the performance defects of the solid electrolyte interphase (SEI) film being particularly prominent.
[0003] The electrolyte interphase (SEI) film, formed on the electrode surface by electrolyte decomposition, is crucial for protecting electrode materials and suppressing side reactions. However, the SEI film in sodium-ion batteries is typically non-uniform, poorly dense, and lacks sufficient thermodynamic stability, making it prone to dissolution or remodeling during charge and discharge. This instability leads to the continuous consumption of electrolyte active components and electrode materials, resulting in poor high-temperature storage and degraded high-temperature cycling performance in sodium-ion batteries. Furthermore, at low temperatures, the unstable SEI film fails to effectively protect the electrodes, causing a decline in low-temperature cycling performance. Therefore, existing sodium-ion batteries exhibit unsatisfactory high-temperature storage and high / low-temperature cycling performance.
[0004] Therefore, there is an urgent need for a non-aqueous electrolyte and a sodium-ion battery containing the non-aqueous electrolyte to address the shortcomings of existing technologies. Summary of the Invention
[0005] In view of the above problems, the purpose of the present invention is to provide a non-aqueous electrolyte and a sodium-ion battery containing the non-aqueous electrolyte, which can significantly improve the high-temperature storage performance and high and low temperature cycling performance of sodium-ion batteries.
[0006] To achieve the above objectives, the present invention provides a non-aqueous electrolyte comprising a non-aqueous organic solvent, a sodium salt, and an additive, wherein the additive comprises compound A and compound B, compound A comprises at least one of the compounds shown in formula 1 and formula 2, and the structure of compound B is shown in formula 3.
[0007] R1 to R2 are each independently selected from hydrogen, cyano, or C1 to C10 hydrocarbon groups, and R3 is selected from C1 to C10 hydrocarbon groups.
[0008] Compared with the prior art, the non-aqueous electrolyte of the present invention uses compounds A and B as additives. Compounds A and B work synergistically to form a uniform, dense, and thermodynamically stable SEI film on the negative electrode surface. At the same time, this SEI film is also rich in high content of inorganic sodium salts (NaF, Na3N, Na2S, N-SO4). x (etc.), which can effectively alleviate the dissolution of the SEI film during high-temperature storage and cycling, thereby improving low-temperature cycling performance and high-temperature storage performance.
[0009] Furthermore, the C1 to C10 hydrocarbon groups of the present invention refer to hydrocarbon groups such as alkyl, alkenyl, alkynyl or aryl groups composed of 1 to 10 carbon atoms; specifically, they may be, but are not limited to, methyl, ethyl, n-propyl, isopropyl, heptyl, octyl, vinyl, allyl, ethynyl, phenyl, benzyl, etc.
[0010] Furthermore, R1 to R2 of the present invention are each independently selected from hydrogen, cyano or C1 to C6 alkyl; R3 is selected from C1 to C6 alkyl, C2 to C5 alkenyl, phenyl or benzyl.
[0011] Furthermore, compound A of the present invention includes at least one of compounds 1 to 8:
[0012]
[0013] .
[0014] Furthermore, the mass percentage of compound A in the non-aqueous electrolyte is 0.5% to 2.0%. Specifically, the mass percentage of compound A in the non-aqueous electrolyte may be, but is not limited to, 0.5%, 0.8%, 1.2%, 1.5%, 1.8%, or 2%.
[0015] Furthermore, the mass percentage of compound B in the non-aqueous electrolyte is 0.1% to 0.5%. Specifically, the mass percentage of compound B in the non-aqueous electrolyte may be, but is not limited to, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5%.
[0016] Furthermore, compound B (NaFMDFB) of the present invention can be prepared by referring to the following synthetic route: .
[0017] Furthermore, the sodium salt of the present invention is selected from at least one of sodium hexafluorophosphate (NaPF6), sodium perchlorate (NaClO4), sodium tetrafluoroborate (NaBF4), sodium trifluoromethanesulfonate (NaCF3SO3), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium bis(oxalate-borate)borate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorooxalate-borate (NaDFOB), sodium difluorodioxalate-phosphate (NaDFOP), and sodium bis(fluorosulfonyl)imide (NaFSI).
[0018] Furthermore, the mass percentage of the sodium salt in the non-aqueous electrolyte of the present invention is 6-16%. Specifically, the mass percentage of the sodium salt in the non-aqueous electrolyte may be, but is not limited to, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, and 16%.
[0019] Furthermore, the non-aqueous organic solvent of the present invention is selected from at least one of chain carbonates, cyclic carbonates and carboxylic acid esters.
[0020] Furthermore, the non-aqueous organic solvent of the present invention is selected from at least one of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (BA), propyl propionate (PP), ethyl propionate (EP), and ethyl butyrate (EB).
[0021] Furthermore, the mass percentage of the non-aqueous organic solvent in the non-aqueous electrolyte of the present invention is 84-92%. Specifically, the mass percentage of the non-aqueous organic solvent in the non-aqueous electrolyte may be, but is not limited to, 84%, 85%, 87%, 88%, 89%, 90%, 91%, or 92%.
[0022] Accordingly, the present invention also provides a sodium-ion battery, including a positive electrode, a negative electrode, and the aforementioned non-aqueous electrolyte. This sodium-ion battery exhibits good high-temperature storage performance and high- and low-temperature cycling performance, which is of great significance for promoting the industrialization of sodium-ion batteries in different application scenarios.
[0023] Furthermore, the active material of the positive electrode in this invention is selected from layered oxides or polyanionic phosphate systems, wherein the chemical formula of the layered oxide is Na. x M (1-y-z) Fe y Mn zO2, wherein M includes at least one of Co, Ni, Cu, Mg, Zn, Al, Sn, Ga, Cr, Sr, V and Ti, 0<x≤1, 0<y<1, 0<z<1, y+z≤1, and the chemical formula of the polyanionic phosphate system is Na4Fe3(PO4)2P2O7. Preferably, the active material of the positive electrode is Na4Fe3(PO4)2P2O7.
[0024] Further, the active material of the negative electrode of the present invention includes at least one of a carbon-based material, a titanium-based structural material and an alloy-type material. Further, the active material of the negative electrode may include hard carbon, soft carbon, sodium titanate, Sb alloy, Sn alloy, potassium alloy, aluminum alloy, copper alloy, molybdenum alloy and the like. Preferably, the active material of the negative electrode is hard carbon. DETAILED DESCRIPTION
[0025] To better illustrate the purpose, technical solutions and beneficial effects of the present invention, the present invention will be further described below with reference to specific examples. It should be noted that the methods described in the following examples are further illustrative of the present invention and should not be construed as limiting the present invention.
[0026] Example 1 (1) Preparation of non-aqueous electrolyte: In a dry argon atmosphere glove box (water content <1ppm), propylene carbonate (PC), ethyl methyl carbonate (EMC) and ethyl butyrate (EB) were mixed at a weight ratio of PC:EMC:EB=7:4:2 to obtain 84.7g of a non-aqueous organic solvent, then 1g of Compound 1 and 0.3g of Compound B (NaFMDFB) were added, after dissolving and fully stirring, 14g of sodium hexafluorophosphate was added, and the mixture was uniformly mixed to obtain the non-aqueous electrolyte.
[0027] (2) Preparation of positive electrode sheet: The polyanionic phosphate material Na4Fe3(PO4)2P2O7, the binder PVDF and the conductive agent SuperP were uniformly mixed at a mass ratio of 95:1:4 to prepare a positive electrode slurry for sodium-ion batteries with a certain viscosity, the prepared slurry was coated on both sides of an aluminum foil, and then dried and rolled to obtain the positive electrode sheet.
[0028] (3) Preparation of negative electrode sheet: Hard carbon, the conductive agent SuperP, the thickener CMC and the binder SBR (styrene-butadiene rubber emulsion) were prepared into a slurry at a mass ratio of 95:1.5:1.0:2.5, mixed uniformly, the prepared slurry was coated on both sides of a copper foil, and then dried and rolled to obtain the negative electrode sheet.
[0029] (4) Preparation of sodium-ion battery: The positive electrode, separator, and negative electrode are stacked to form a square cell, which is then packaged with polymer and filled with the sodium-ion battery non-aqueous electrolyte prepared above. After formation, capacity testing and other processes, a sodium-ion battery with a capacity of 1300mAh is produced.
[0030] The non-aqueous electrolyte formulations of Examples 1-12 and Comparative Examples 1-3 are shown in Table 1. The steps for preparing the non-aqueous electrolyte and the sodium-ion battery in Examples 2-12 and Comparative Examples 1-3 are the same as those in Example 1.
[0031] Table 1 Electrolyte Components of Each Example and Comparative Example
[0032] The sodium-ion batteries prepared in Examples 1-12 and Comparative Examples 1-3 were tested for initial efficiency, low-temperature cycle performance, high-temperature cycle performance, and high-temperature storage performance, respectively. The specific test conditions are as follows, and the test results are shown in Table 2.
[0033] (1) First Coulomb efficiency test Sodium-ion batteries were placed in a high-temperature, high-pressure formation chamber and formed in three steps at 25°C and 0.28 MPa (4 cells). The first step involved a constant current of 0.05C for 60 minutes, recording the charging capacity C1. The second step involved a constant current of 0.1C for 120 minutes, recording the charging capacity C2. The third step involved a constant current of 0.2C for 240 minutes, recording the charging capacity C3. The upper limit voltage was 3.6V. The batteries were then resealed using a rotary sealing machine. They were then charged at room temperature at a constant current of 0.5C until the voltage reached 3.6V, followed by constant voltage charging at 3.6V until the current reached 0.05C, and finally constant current discharging at 1C until the voltage reached 1.5V. The initial discharge capacity C0 was recorded, and the initial coulombic efficiency was calculated as C0 / (C1+C2+C3)×100%.
[0034] (2) Low-temperature cycling performance test At room temperature (25℃), the sodium-ion battery was charged and discharged once at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 3.6V. The battery was then placed in a low-temperature chamber at -10℃ and discharged at a constant current of 0.1C until the voltage reached 1.5V. The first discharge capacity of the battery was recorded. This constitutes one charge-discharge cycle. After 20 cycles, the battery was disassembled, and the presence of sodium deposits on the electrodes was observed and the capacity retention rate was calculated.
[0035] Capacity retention rate = (Discharge capacity in the last cycle / Discharge capacity in the first cycle) × 100% (3) High-temperature cycling performance test The sodium-ion battery was placed in a 55°C constant temperature chamber and allowed to stand for 30 minutes to reach a constant temperature. It was then charged at a constant current of 1C until the voltage reached 3.6V, followed by a constant voltage charge of 3.6V until the current reached 0.05C. Finally, it was discharged at a constant current of 1C until the voltage reached 1.5V. The discharge capacity of the battery in the first cycle was recorded; this constitutes one charge-discharge cycle. This cycle was repeated 400 times, recording the discharge capacity of the first and last cycles. The capacity retention rate was calculated using the following formula.
[0036] Capacity retention rate = (Discharge capacity in the last cycle / Discharge capacity in the first cycle) × 100% (4) High-temperature storage performance test: Under normal temperature (25℃) conditions, a sodium-ion battery was subjected to one 0.5C / 0.5C charge and discharge cycle (battery discharge capacity recorded as C0), with an upper limit voltage of 3.6V. Then, the battery was charged to 3.6V under constant current and constant voltage conditions at 0.5C. The battery was placed in a 60℃ oven for 30 days, then removed and placed in a 25℃ environment for 0.5C discharge, with the discharge capacity recorded as C1. The sodium-ion battery was then subjected to one 0.5C / 0.5C charge and discharge cycle (battery discharge capacity recorded as C2). The capacity retention rate and capacity recovery rate of the sodium-ion battery were calculated using the following formulas: Capacity retention rate = (C1 / C0) × 100% Capacity recovery rate = (C2 / C0) × 100% Table 2 Performance test results of sodium-ion batteries in each embodiment and comparative example
[0037] As shown in Table 1, the sodium-ion batteries of Examples 1-12 exhibit better initial coulombic efficiency, low-temperature performance, high-temperature cycle performance, and high-temperature storage performance than Comparative Example 1. This is because the non-aqueous electrolyte of this invention uses compounds A and B as additives. Compounds A and B, through synergistic effects, can form a uniform, dense, and thermodynamically stable SEI film on the negative electrode surface. Furthermore, this SEI film is rich in high amounts of inorganic sodium salts (NaF, Na3N, Na2S, N-SO4). x (etc.), which can effectively alleviate the dissolution of the SEI film during storage and cycling, thereby improving low-temperature cycling performance and storage performance.
[0038] Comparing Example 8 and Comparative Example 2, it can be seen that the sodium-ion battery of Example 8 has better initial coulombic efficiency, low-temperature performance, high-temperature cycle performance, and high-temperature storage performance than Comparative Example 2. This is because the fluorine content of the SEI film surface layer of the sodium-ion battery of Comparative Example 2 decreases significantly after high-temperature storage. The main reason for this is the continuous dissolution and formation of the SEI film during storage, which leads to the thickening of the SEI film. Furthermore, the newly formed SEI on the surface is mainly composed of organic components, which masks most of the inorganic fluorine-containing sodium salts in the inner layer, further reducing its electronic insulation capacity. This will further accelerate the solvent by-decomposition reaction until the SEI film grows to a certain thickness. However, in Example 8, compounds A and B can form a uniform, dense, and thermodynamically stable SEI film on the negative electrode surface through synergistic effects. This film has a high content of inorganic sodium salts NaF, Na3N, Na2S, and N-SO4. x These methods can effectively alleviate the dissolution of SEI during storage and cycling. The newly generated SEI on the surface is still mainly composed of inorganic components, thereby improving low-temperature cycling performance and high-temperature storage performance.
[0039] Comparing Example 8 and Comparative Example 3, it can be seen that the sodium-ion battery of Example 8 has better initial coulombic efficiency, low-temperature performance, high-temperature cycle performance, and high-temperature storage performance than Comparative Example 3. This is because when NaFMDFB is used alone, a boron-containing CEI / SEI film is formed on the electrode surface. During storage, the SEI film is continuously dissolved and generated, resulting in the SEI film thickening. Moreover, the newly generated SEI on the surface is mainly composed of organic components, which leads to performance deterioration.
[0040] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A non-aqueous electrolyte, comprising a non-aqueous organic solvent, a sodium salt, and additives, characterized in that, The additive includes compound A and compound B, wherein compound A includes at least one of the compounds shown in Formula 1 and Formula 2, and the structure of compound B is shown in Formula 3. R1 to R2 are each independently selected from hydrogen, cyano, or C1 to C10 hydrocarbon groups, and R3 is selected from C1 to C10 hydrocarbon groups.
2. The non-aqueous electrolyte as described in claim 1, characterized in that, R1 to R2 are each independently selected from hydrogen, cyano, or C1 to C6 alkyl; R3 is selected from C1 to C6 alkyl, C2 to C5 alkenyl, phenyl, or benzyl.
3. The non-aqueous electrolyte as described in claim 1, characterized in that, Compound A includes at least one of compounds 1 to 8: 。 4. The non-aqueous electrolyte as described in claim 1, characterized in that, The mass percentage of compound A in the non-aqueous electrolyte is 0.5-2.0%.
5. The non-aqueous electrolyte as described in claim 1, characterized in that, The mass percentage of compound B in the non-aqueous electrolyte is 0.1~0.5%.
6. The non-aqueous electrolyte as described in claim 1, characterized in that, The sodium salt is selected from at least one of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium trifluoromethanesulfonate, sodium bis(trifluoromethanesulfonyl)imide, sodium bis(oxalate-borate), sodium difluorophosphate, sodium di(oxalate-borate), sodium di(oxalate-difluorophosphate), and sodium bis(oxalate-imide).
7. The non-aqueous electrolyte as described in claim 1, characterized in that, The non-aqueous organic solvent is selected from at least one of chain carbonates, cyclic carbonates, and carboxylic acid esters.
8. The non-aqueous electrolyte as described in claim 7, characterized in that, The non-aqueous organic solvent is selected from at least one of ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, propylene carbonate, butyl acetate, propyl propionate, ethyl propionate, and ethyl butyrate.
9. A sodium-ion battery, comprising a positive electrode and a negative electrode, characterized in that, It also includes the non-aqueous electrolyte as described in any one of claims 1 to 8.
10. The sodium-ion battery as described in claim 9, characterized in that, The active material of the positive electrode is selected from a layered oxide of the chemical formula Na x M (1-y-z) Fe y Mn z O2, wherein M comprises at least one of Co, Ni, Cu, Mg, Zn, Al, Sn, Ga, Cr, Sr, V and Ti, 0 < x < 1, 0 < y < 1, 0 < z < 1, y + z < 1, and a polyanionic phosphate system of the chemical formula Na4Fe3(PO4)2P2O7, the active material of the negative electrode comprising at least one of a carbon-based material, a titanium-based structural formula and an alloy-based material.
Citation Information
Patent Citations
Battery monomer, battery and electric device
CN118213597A
Electrolyte solution for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery containing same
WO2024253162A1