A battery separator and its preparation method, and a secondary battery

By intermittently coating polymer coatings of different areas and pore sizes on both sides of the positive and negative electrodes of the lithium-ion battery separator, the problems of rapid electrolyte consumption and dendrite precipitation are solved, achieving high electrolyte retention capacity and long-life fast-charging performance of the battery.

CN120637792BActive Publication Date: 2026-11-17ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510829135.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-20
Publication Date
2026-11-17
Estimated Expiration
2045-06-20

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators consume electrolyte too quickly during fast charging, resulting in short cell cycle life, metal dendrite precipitation, and affecting safety and battery performance.

Method used

Polymer coatings with different areas and pore sizes are intermittently coated on both sides of the positive and negative electrodes of the separator substrate. The area ratio and pore size distribution of coating A and coating B are designed to meet the adhesion and liquid retention requirements of different sides, thereby improving the liquid retention and ion conduction efficiency of the cell.

Benefits of technology

It improves the battery's liquid retention capacity, reduces dendrite precipitation, extends the battery's fast-charge cycle life, and ensures the battery's high ion conduction efficiency and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120637792B_ABST
    Figure CN120637792B_ABST
Patent Text Reader

Abstract

This application discloses a battery separator, its preparation method, and a secondary battery, relating to the field of battery separators. The battery separator includes a separator substrate, with a polymer coating A on its surface A near the positive electrode and a polymer coating B on its surface B near the negative electrode. The area ratio of polymer coating A to surface A is 60%-85%, with an average pore size of 1-1.6 μm; the area ratio of polymer coating B to surface B is 70%-90%, with an average pore size of 0.4-1.3 μm. This application achieves this by intermittently coating polymer coatings on both sides of the separator, with adjacent coating bands forming grooves to increase electrolyte storage space. By combining this with the design of different average pore sizes and coating areas on both sides of the polymer coating, the different adhesion and electrolyte retention requirements of the separator on the positive and negative electrode surfaces are simultaneously met, thus achieving a balance between improving battery electrolyte retention, cell expansion, and capacity retention during fast charging cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery separators, and more particularly to a battery separator, a method for preparing the separator, and a secondary battery. Background Technology

[0002] In recent years, the rapid growth of new energy vehicles and portable electronic devices has placed increasingly higher demands on the fast charging and discharging performance of batteries. The ion conduction efficiency of the separator directly affects the fast charging and discharging performance of the battery. Currently, commonly used lithium-ion battery separators are generally ceramic separators, coated with adhesive polymers such as PVDF or PMMA to form an adhesive layer, improving the adhesion between the separator and the positive and negative electrodes, thereby improving the performance of the cell. The average pore size of conventional oil-based PVDF coatings is less than 0.5μm, and the pore size of the PVDF coatings on both sides of the substrate is also designed to be the same, resulting in low porosity of the polymer coating. During fast charging, lithium batteries using the above-mentioned separators experience excessive electrolyte consumption and insufficient electrolyte retention, leading to a short cycle life of the cell. This may also affect the precipitation of metal dendrites on the negative electrode, impacting cycle life and safety. Sharp dendrites, once they grow to a certain size, can pierce the separator, thus affecting safety. In lithium-ion batteries, the precipitation of metal dendrites is known as lithium plating.

[0003] Short battery cycle life, meaning a rapid decline in capacity retention, is largely due to the rapid electrolyte consumption during fast charging. Simultaneously, electrode expansion reduces the gap between electrodes, leading to insufficient electrolyte retention in the later stages of cycling and a drop in cycle life. Furthermore, the areas of greatest expansion stress in the battery cell are the corner regions, where electrolyte consumption is most significant, and the risk of dendrite formation is particularly pronounced. Therefore, developing separators with high electrolyte retention and improved dendrite formation resistance is of great importance. Summary of the Invention

[0004] This application provides a battery separator, its preparation method, and a secondary battery. By intermittently coating a polymer coating on both sides of the separator substrate and designing different pore sizes on both sides of the polymer coating, the different adhesion and liquid retention requirements of the separator on the positive and negative electrode surfaces can be met simultaneously, thereby improving the liquid retention capacity and ion conduction efficiency of the battery cell. This approach aims to improve the battery's liquid retention, cell expansion, dendrite formation, and capacity retention during fast charging cycles.

[0005] To address the aforementioned technical problems, one objective of this application is to provide a battery separator, comprising a separator substrate, wherein the separator substrate includes a surface A near the positive electrode and a surface B near the negative electrode, wherein a polymer coating A is provided on surface A and a polymer coating B is provided on surface B;

[0006] The polymer coating A comprises at least two spaced-apart coating strips A, and the ratio S of the area of ​​the polymer coating A to the area of ​​the surface A is...A It ranges from 60% to 85%;

[0007] The polymer coating B comprises at least two spaced-apart coating strips B, and the ratio S of the area of ​​the polymer coating B to the area of ​​the surface B is... B It is 70%-90%;

[0008] The angles formed by the coating strip A, the coating strip B and the length direction of the diaphragm substrate are independent, and one of the angles is an acute angle;

[0009] Both polymer coating A and polymer coating B contain micropores, and the average pore size P of the micropores in polymer coating A is... A The pore size is 1-1.6 μm, and the pore size is (P A -0.1)~(P A Pore ​​size distribution rate D (+0.1) μm A ≥80%; the average pore size P of the micropores contained in the polymer coating B B The micrometer size is 0.4-1.3 μm, and the pore size is (P B -0.1)~(P B Pore ​​size distribution rate D (+0.1) μm B ≥80%;

[0010] The S A S B P A P B D A D B The following relationship exists between them:

[0011] M A =S A ×P A ×D A M B =S B ×P B ×D B And 0.5≤M A / M B ≤3.5.

[0012] This application provides a battery separator with high electrolyte retention and high ionic conductivity. Polymer coatings A and B are intermittently disposed on surfaces A and B of the battery separator, respectively. By controlling the relationship between the coating area ratio on the separator substrate surface and the formed pore size, the adhesion requirements of the polymer coating can be met, ensuring the high porosity and high ionic conductivity of the battery separator. At the same time, some uncoated areas are reserved on the surface of the separator substrate to form intermittent grooves, which can increase the electrolyte storage space, improve the electrolyte retention capacity of the battery, reduce the consumption of circulating electrolyte in the corner area of ​​the battery, and alleviate the dendrite precipitation phenomenon in the negative electrode material area.

[0013] In this process, polymer coating A faces the positive electrode of the battery, while polymer coating B faces the negative electrode. Since the expansion of the positive electrode is less than that of the negative electrode, the adhesive force of polymer coating B needs to be higher than that of polymer coating A in order to suppress cell expansion. To ensure a greater adhesive force, a larger amount of polymer coating is usually required, which reduces the porosity and liquid retention capacity of the micropores. Therefore, by simultaneously increasing the porosity or pore size of polymer coating A, it is possible to suppress cell expansion while obtaining high liquid retention capacity. This application controls the average pore size of polymer coating A to be above 1 μm and the average pore size of polymer coating B to be above 0.4 μm, which helps to further improve the liquid retention capacity of the battery, reduce dendrite precipitation in the negative electrode area, and effectively improve the cycle capacity retention rate of the cell. However, if the average pore size of the polymer coating is too large, the adhesion of the polymer coating will decrease. Therefore, controlling the average pore size of polymer coating A to be below 1.6 μm and the average pore size of polymer coating B to be below 1.3 μm can effectively ensure the adhesion of the coating, improve the ion conduction efficiency of the separator, and avoid excessive expansion of the cell during cycling. Meanwhile, the pore size is (P... A -0.1)~(P A +0.1)μm and (P B -0.1)~(P B A pore size distribution rate of +0.1)μm ≥80% can ensure the uniformity of the polymer coating pore size, which is beneficial to the good consistency of coating adhesion and liquid retention capacity in various regions of the separator, thereby ensuring the stability of cell performance.

[0014] Furthermore, when the polymer coating area of ​​the battery separator in this application is less than 60%, the adhesion of the coating decreases, the cell expansion rate increases, and the cell's electrolyte retention capacity weakens. When the polymer coating area is greater than 90%, the uncoated portion of the separator substrate surface is small, and the resulting intermittent grooves cannot effectively store electrolyte, leading to poor electrolyte retention capacity of the separator, dendrite precipitation on the negative electrode, and low cell cycle capacity retention. Therefore, controlling the polymer coating area within the range of 60%-90% can simultaneously improve the battery's electrolyte retention, cell expansion, and capacity retention, thereby extending the battery's fast-charge cycle life.

[0015] This application controls S A S B P A P B D A D B The relationship between them is 0.5 ≤ M A / M B A value ≤3.5 allows for an optimal balance between cell expansion suppression and cycle liquid retention. If M... A / MB If the ratio is less than 0.5, the adhesion of polymer coating B is too poor, leading to excessive cell expansion; if M A / M B A ratio greater than 3.5 indicates that although cell expansion is relatively small, the risk of lithium plating is relatively high.

[0016] As a preferred embodiment, the average pore size P of the polymer coating A A The range is any one or any two of the following: 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, and 1.6μm.

[0017] As a preferred embodiment, the average pore size P of the polymer coating B is... B It is a range of any one or any two of the following: 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, and 1.3μm.

[0018] As a preferred embodiment, the average pore size P of the polymer coating A A The average pore size P of the polymer coating B is 1.2-1.4 μm. B It is 0.6-0.8μm.

[0019] As a preferred embodiment, the ratio S of the area of ​​the polymer coating A to the area of ​​the surface A is... A The range is any one or any two of 60%, 65%, 70%, 75%, 80%, and 85%.

[0020] As a preferred embodiment, the ratio S of the area of ​​the polymer coating B to the area of ​​the surface B is... B The range is any one or any two of 70%, 75%, 80%, 85%, and 90%.

[0021] As a preferred embodiment, the ratio S of the area of ​​the polymer coating A to the area of ​​the surface A is... A The ratio S of the area of ​​the polymer coating B to the area of ​​the surface B is 65%-75%. B It is 75%-85%.

[0022] When the average pore size and coating area of ​​polymer coating A and polymer coating B on the separator are controlled within the above-mentioned range, this application can further improve the liquid retention, cell expansion, and capacity retention of the battery. The larger average pore size of the double-sided polymer coating, combined with the appropriate coating area, can effectively improve the liquid retention capacity of the cell, improve the liquid retention capacity of the cell corner area, and reduce dendrite precipitation. At the same time, the average pore size and coating area of ​​the polymer coating within the above-mentioned range can meet the adhesion requirements of different surfaces of the separator, so as to further reduce cell expansion. Moreover, the battery can maintain a high capacity retention rate during fast charging cycle, thus improving fast charging performance.

[0023] As a preferred embodiment, the polymer coating A is formed by coating and drying a polymer coating slurry A, wherein the polymer coating slurry A comprises solvent A1 and solvent A2 in a mass percentage ratio of (84-92):(8-16);

[0024] The polymer coating B is formed by coating and drying a polymer coating slurry B, wherein the polymer coating slurry B comprises solvent B1 and solvent B2 in a mass percentage of (88-95):(5-12).

[0025] Solvents A1 and B1 are each independently at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and acetone, and solvents A2 and B2 are each independently at least one of methanol, ethanol, isopropanol, n-butanol, and water.

[0026] As a preferred embodiment, the polymer coating slurry A and the polymer coating solvent B are each independent and also include a polymer with a mass fraction of 8wt%-15wt%.

[0027] As a preferred embodiment, the polymer coating slurry A and the polymer coating solvent B are each independent and further include a polymer with a mass fraction of any one or any two of the following: 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, and 15wt%.

[0028] As a preferred embodiment, the polymers of polymer coating A and polymer coating B are each independent and include at least one of the following: polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trifluoroethylene copolymer, polyvinylidene fluoride-trifluorochloroethylene copolymer, polyvinylidene fluoride-tetrafluoroethylene copolymer, polyvinylidene fluoride-trifluoroethylene-trifluorochloroethylene copolymer, polyvinylidene fluoride-trifluoroethylene-chlorofluoroethylene copolymer, polyetherimide, polyimide, polymethyl methacrylate, para-aramid, meta-aramid, and acrylate copolymer.

[0029] As a preferred embodiment, the thicknesses of polymer coating A and polymer coating B are independent and range from 0.5 to 3 μm.

[0030] As a preferred embodiment, the polymer coating A contains at least two coating strips A distributed in parallel, and the distance between two adjacent coating strips A is 0.2-3 mm, and one of the included angles formed between the coating strip A and the diaphragm substrate along the length direction is 30-60 degrees.

[0031] As a preferred embodiment, the polymer coating B contains at least two coating strips B distributed in parallel, and the distance between two adjacent coating strips B is 0.2-3 mm, and one of the included angles formed between the coating strips B and the diaphragm substrate along the length direction is 30-60 degrees.

[0032] The polymer coating of the battery separator in this application is distributed in strip-shaped strips, which can form an effective gap between adjacent coating strips to store electrolyte. The polymer coating area on both sides of the substrate is different. Combined with the different average pore sizes of polymer coatings A and B, the electrolyte retention capacity of the cell is improved, the cycle capacity retention rate of the cell is increased, and lithium plating and cell expansion are improved simultaneously.

[0033] As a preferred embodiment, the membrane substrate is at least one of polyethylene, polypropylene, polyethylene terephthalate, polyimide, aramid, and poly(terephthalic acid) butylene glycol.

[0034] As a more preferred embodiment, the surface A and / or surface B of the diaphragm substrate are coated with at least one of the following: alumina, boehmite, magnesium oxide, magnesium hydroxide, barium titanate, aluminum hydroxide, silicon dioxide, aluminum nitride, lithium titanium aluminum phosphate, lithium lanthanum zirconium oxide solid electrolyte, melamine cyanurate, melamine polyphosphate, ammonium polyphosphate, triphenyl phosphate, decabromodiphenyl ethane, tetrabromobisphenol A, brominated polystyrene, cellulose, and polyimide.

[0035] As a preferred embodiment, surface A and / or surface B of the diaphragm substrate is a polyethylene wet-process base film coated with boehmite with a thickness of 0.3-3 μm.

[0036] To address the aforementioned technical problems, a second objective of this application is to provide a method for preparing a battery separator, comprising the following steps:

[0037] The polymer coating slurry A is coated on the surface A of the separator substrate, immersed in a coagulation bath and dried to form polymer coating A. The polymer coating slurry B is coated on the surface B of the separator substrate, immersed in a coagulation bath and dried to form polymer coating B, thus obtaining the battery separator.

[0038] This application employs a non-solvent-induced phase separation pore-forming technology, which mainly controls the ratio and type of solvent A1 or B1 to solvent A2 or B2, and also adjusts the composition ratio of the coagulation bath to control the pore size and distribution of the coating.

[0039] As a preferred embodiment, the coagulation bath includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, acetone, ethanol, isopropanol, n-butanol, and water.

[0040] As a preferred option, the soaking time in the coagulation bath is 1-20 minutes.

[0041] As a preferred option, the drying temperature is 50-90℃ and the time is 1-30 minutes.

[0042] To address the aforementioned technical problems, a third objective of this application is to provide a secondary lithium-ion battery, comprising a positive electrode, a negative electrode, an electrolyte, and a battery separator.

[0043] As a preferred embodiment, the positive electrode sheet includes an aluminum foil and a positive electrode material coated on both sides of the aluminum foil. The positive electrode material includes a positive electrode active material, a conductive agent, and a binder A in a mass ratio of (94-98):(1-2):(1-2).

[0044] As a preferred embodiment, the positive electrode active material is at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, and lithium manganese iron phosphate.

[0045] As a preferred embodiment, the conductive agent is at least one of conductive carbon black, conductive graphite, carbon nanotubes, acetylene black, and graphene.

[0046] As a preferred embodiment, the adhesive A is at least one of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, ethylene-tetrafluoroethylene copolymer, and ethylene trifluorochloroethylene.

[0047] As a preferred embodiment, the negative electrode sheet includes a copper foil and a negative electrode material coated on both sides of the copper foil. The negative electrode material includes a negative electrode active material in a mass ratio of (96-99):(0.5-2):(0.5-2), binder B, and sodium carboxymethyl cellulose.

[0048] As a preferred embodiment, the negative electrode active material is at least one of carbon-based compounds, silicon-based compounds, titanium-based compounds, tin-based alloys, and transition metal nitrides.

[0049] As a preferred embodiment, the negative electrode active material is graphite.

[0050] As a preferred embodiment, the adhesive B is at least one of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, ethylene-tetrafluoroethylene copolymer, and ethylene trifluorochloroethylene.

[0051] As a preferred embodiment, the electrolyte comprises a lithium salt with a concentration of 0.5-3 mol / L and the balance being an organic solvent.

[0052] As a preferred embodiment, the organic solvent is at least one of ethylene carbonate, propylene carbonate, and dimethyl carbonate.

[0053] As a preferred embodiment, the organic solvent comprises ethylene carbonate, propylene carbonate, and dimethyl carbonate in a mass ratio of (2-4):(1-3):(3-5).

[0054] As a preferred embodiment, the lithium salt is lithium hexafluorophosphate.

[0055] As a preferred embodiment, the method for preparing the secondary lithium-ion battery includes the following steps:

[0056] (1) Mix the positive electrode active material, conductive agent and binder, add solvent C and stir evenly to obtain a positive electrode slurry with a solid content of 60wt%-80wt%. Coat the positive electrode slurry on both sides of aluminum foil and dry to obtain a positive electrode sheet.

[0057] (2) Mix the negative electrode active material, binder and sodium carboxymethyl cellulose, add water and stir evenly to obtain a negative electrode slurry with a solid content of 50wt%-70wt%. Coat the negative electrode slurry on both sides of the copper foil and dry to obtain a negative electrode sheet.

[0058] (3) Assemble the positive electrode, battery separator and negative electrode in sequence, roll them up and place them in an aluminum-plastic film packaging bag. After drying, inject electrolyte. After vacuum sealing, standing, formation, degassing and trimming, a secondary lithium-ion battery is obtained.

[0059] As a preferred embodiment, the solvent C is at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0060] As a preferred embodiment, in steps (1) and (2), the drying temperature is 100-130℃ and the time is 1-3h.

[0061] As a preferred embodiment, the electrolyte is prepared by mixing an organic solvent in an argon atmosphere glove box with a water content of <10ppm, and then adding a lithium salt to the organic solvent to obtain the electrolyte.

[0062] To address the aforementioned technical problems, the fourth objective of this application is to provide an electrical device comprising the aforementioned secondary lithium-ion battery.

[0063] The secondary lithium-ion battery of the present invention can be applied to electrical devices that use batteries as power sources or to various energy storage systems that use batteries as energy storage elements. The electrical devices include, but are not limited to, mobile phones, tablet computers, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc.

[0064] Compared with the prior art, this application has the following beneficial effects:

[0065] This application controls the intermittent coating of a polymer coating A covering 60%-85% of the battery separator near the positive electrode and an intermittent coating of a polymer coating B covering 70%-90% of the battery separator near the negative electrode, leaving some uncoated areas to form intermittent grooves. This increases the electrolyte storage space and improves the battery's electrolyte retention capacity. Simultaneously, by combining the different average pore sizes and pore size distributions of polymer coatings A and B, the design balances coating adhesion and electrolyte retention capacity, avoiding situations where excessively large average pore sizes affect adhesion or excessively small average pore sizes affect electrolyte retention. This collaboratively reduces electrolyte consumption in the battery corner areas, alleviates dendrite formation in the negative electrode area, improves the cell's long-cycle capacity retention, ensures high ion conductivity of the battery separator, effectively suppresses cell expansion, and extends fast-charging cycle life. Attached Figure Description

[0066] Figure 1 This is a schematic cross-sectional view of a battery separator in an embodiment of this application;

[0067] Figure 2 This is a top view schematic diagram of a polymer coating in a battery separator according to an embodiment of this application. Detailed Implementation

[0068] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0069] It should be understood that the terminology used in this application is merely for describing particular implementations and is not intended to limit the application. Furthermore, for numerical ranges in this application, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this application. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0070] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art described herein. While only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this application. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0071] As used in this article:

[0072] "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0073] The conjunction "composed of..." excludes any unspecified elements, steps, or components. If used in a claim, this phrase makes the claim closed, excluding materials other than those described, except for associated conventional impurities. When the phrase "composed of..." appears in a clause of the body of a claim rather than immediately following it, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0074] In the description of this application, it should be understood that the terms "upper", "lower", "left", "right", "top", "bottom", etc., indicating the orientation or positional relationship, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0075] To further illustrate this application, the following detailed description is provided in conjunction with embodiments, but these should not be construed as limiting the scope of protection of this application. Unless otherwise specified, the raw materials used in the following embodiments and comparative examples are commercially available, and the same raw materials were used in parallel experiments.

[0076] Examples 1-10 and Comparative Examples 1-9

[0077] A battery separator includes a separator substrate, the separator substrate having a surface A near the positive electrode and a surface B near the negative electrode, the surface A being coated with a polymer coating A and the surface B being coated with a polymer coating B.

[0078] like Figure 1-2 As shown, the polymer coating A comprises at least two spaced-apart coating strips A, and the ratio of the area of ​​the polymer coating A to the area of ​​the surface A is S. A As shown in Table 1, the polymer coating B comprises at least two spaced-apart coating strips B, and the ratio of the area of ​​the polymer coating B to the area of ​​the surface B is S. B The details are shown in Table 1.

[0079] Both polymer coating A and polymer coating B contain micropores, and the average pore size of the micropores in polymer coating A is P. A And the aperture is (P) A -0.1)~(P A Pore ​​size distribution rate D (+0.1) μm A ≥90%; the average pore size of the micropores contained in polymer coating B is P B And the aperture is (P) B -0.1)~(P B Pore ​​size distribution rate D (+0.1) μm B ≥90%, as shown in Table 1; the above S A S B P A P B D A D B The following relationship exists between them:

[0080] M A =S A ×P A ×D A M B =S B ×P B ×D B Examples 1-10 satisfy 0.5 ≤ M A / M B ≤3.5;

[0081] The thickness of polymer coating A and polymer coating B is 1 μm. The spacing between adjacent coating strips A and B is 1 mm. The included angle between coating strip A, coating strip B and the membrane substrate along the length direction is 45 degrees.

[0082] The above-mentioned method for preparing a battery separator includes the following steps:

[0083] (1) Polyvinylidene fluoride-hexafluoropropylene copolymer (Arkema, France, brand name LBG) was added to N,N-dimethylacetamide (DMAC), stirred and dissolved at 60°C, and then ethanol was added. The mass percentages of DMAC and ethanol are shown in Table 1. The mixture was stirred until completely dissolved to obtain polymer coating slurry A with a polyvinylidene fluoride-hexafluoropropylene copolymer mass concentration of 10 wt%. Polyvinylidene fluoride-hexafluoropropylene copolymer was added to DMAC, stirred and dissolved at 60°C, and then ethanol was added. The mass percentages of DMAC and ethanol are shown in Table 1. The mixture was stirred until completely dissolved to obtain polymer coating slurry B with a polyvinylidene fluoride-hexafluoropropylene copolymer mass concentration of 10 wt%.

[0084] (2) The polymer coating slurry A is uniformly coated on the surface A of the diaphragm substrate by intermittent coating. Then it is immersed in deionized water at 25°C for 3 min and then dried at 60°C for 20 min to form polymer coating A. The average pore size of polymer coating A is shown in Table 1 below.

[0085] The membrane substrate is a polyethylene wet-process base membrane that has been pre-coated with 1μm thick boehmite on both sides.

[0086] (3) The polymer coating slurry B is uniformly coated on the surface B of the separator substrate by intermittent coating. Then it is immersed in deionized water at 25°C for 3 min and then dried at 60°C for 20 min to form the polymer coating B. The battery separator is prepared. The average pore size of the polymer coating B is shown in Table 1 below.

[0087] Comparative Example 10

[0088] A battery separator is prepared in a manner that uses the same reagents, equipment and process parameters as in Example 1. The difference is that in step (2), the surface A of the separator substrate is not coated with polymer coating slurry A.

[0089] Comparative Example 11

[0090] A battery separator is prepared in a manner that uses the same reagents, equipment and process parameters as in Example 1. The difference is that in step (3), the surface B of the separator substrate is not coated with polymer coating slurry B.

[0091] Comparative Example 12

[0092] A battery separator is prepared in a manner that uses the same reagents, equipment and process parameters as in Example 1. The difference is that in steps (2) and (3), coating strip A and coating strip B are respectively arranged parallel to the separator substrate along the length direction.

[0093] Comparative Example 13

[0094] A battery separator is prepared in a manner that uses the same reagents, equipment and process parameters as in Example 1. The difference is that in steps (2) and (3), coating strip A and coating strip B are respectively set perpendicular to each other along the length direction of the separator substrate.

[0095] Table 1 - Polymer coating raw materials and coating area percentage of battery separators in the examples and comparative examples

[0096]

[0097]

[0098] Application Example 1-10 and Comparative Application Example 1-13

[0099] A secondary battery includes a positive electrode, a negative electrode, a battery separator, and an electrolyte, wherein the battery separator is the battery separator prepared in Examples 1-10 or Comparative Examples 1-13;

[0100] The positive electrode sheet includes aluminum foil and positive electrode material coated on both sides of the aluminum foil. The aluminum foil is 8μm thick and the positive electrode size is 65mm×860mm. The positive electrode material includes lithium cobalt oxide, carbon black and polyvinylidene fluoride in a mass ratio of 97:1.5:1.5.

[0101] The negative electrode sheet includes copper foil and negative electrode material coated on both sides of the copper foil. The thickness of the copper foil is 6μm, the negative electrode size is 69mm×868mm, and the negative electrode material includes graphite, styrene-butadiene rubber and sodium carboxymethyl cellulose in a mass ratio of 98:1:1.

[0102] The electrolyte consists of 1 mol / L lithium hexafluorophosphate and the remainder organic solvent, which includes ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) in a mass ratio of 3:2:4.

[0103] The above-mentioned method for preparing a secondary battery includes the following steps:

[0104] (1) Lithium cobalt oxide, carbon black and polyvinylidene fluoride were mixed in a mass ratio of 97:1.5:1.5, N-methylpyrrolidone was added, and the mixture was stirred evenly under vacuum stirring to obtain a positive electrode slurry with a solid content of 75wt%. The positive electrode slurry was evenly coated on both sides of aluminum foil and dried at 125℃ for 2h. After cold pressing, cutting and slitting, the positive electrode sheet was obtained.

[0105] (2) Graphite, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 98:1:1, deionized water is added, and the mixture is stirred evenly under the action of a vacuum mixer to obtain a negative electrode slurry with a solid content of 60wt%. The negative electrode slurry is evenly coated on both sides of copper foil and dried at 120℃ for 2h. After cold pressing, cutting and slitting, a negative electrode sheet is obtained.

[0106] (3) In an argon atmosphere glove box with a water content of <10ppm, EC, PC and DMC are mixed in a mass ratio of 3:2:4 to obtain an organic solvent, and then lithium hexafluorophosphate is added to the organic solvent to obtain an electrolyte.

[0107] (4) Assemble the positive electrode, battery separator and negative electrode in sequence, so that the battery separator is in the middle of the positive electrode and the negative electrode to play a role in isolation. Wrap the electrode assembly to obtain the electrode assembly, place the electrode assembly in an aluminum-plastic film packaging bag, dry it and inject electrolyte. After vacuum sealing, standing, formation, degassing and trimming, a secondary battery is obtained.

[0108] Performance testing

[0109] 1. Test method for polymer coating pore size of battery separator in the examples and comparative examples: A range of one meter was selected on the surface of the battery separator, and three samples were randomly selected from the range. The surface morphology of the samples was observed and photographed by scanning electron microscopy. The pore size of the coating in the photographs was analyzed by scanning electron microscopy analysis software. The pore size of all micropores was measured, and the average pore size and pore size distribution rate were calculated. The test results are shown in Table 1.

[0110] 2. Battery charge-discharge cycle test: The lithium-ion batteries prepared in the application example and the comparative application example were placed in an environment of 25°C and left to stand for 30 minutes. Then, they were charged at a constant current of 4C to 4.50V, and then charged at a constant voltage of 4.50V to 0.05C. After standing for 5 minutes, they were discharged at a constant current of 0.7C to 3.0V. The charge-discharge cycle was repeated 800 times. The capacity retention rate and cell thickness expansion rate (PPG test, full charge to full charge) of the battery after 800 cycles at room temperature and 4C were tested. The lithium deposition in the negative electrode area was observed. The method for determining the lithium deposition level is shown in Table 2. The test results are shown in Table 3.

[0111] Table 2 - Methods for Determining Lithium Plating Grade in Anode Material Regions

[0112]

[0113] Table 3 - Battery charge-discharge cycle test results for application examples and comparative application examples

[0114]

[0115]

[0116] As shown in Table 3, in Examples 1-3 and 8-9, the average pore size of polymer coating A on the diaphragm is 1-1.6 μm, and that of polymer coating B is 0.7-1.3 μm, and both satisfy 0.5 ≤ M. A / M B ≤3.5 μm indicates that the battery capacity retention rate is above 82%, the cell expansion rate is low, and there is no lithium plating or only trace amounts of lithium plating in the negative electrode area. This demonstrates that when the pore sizes of both sides of the separator are within the above range, it is possible to simultaneously improve battery capacity retention, cell expansion, and lithium plating. In contrast, the polymer coating A of the separators in Comparative Examples 1 and 3-4 has a lower average pore size of 0.5 μm. Since separator A faces the positive electrode and separator B faces the negative electrode, side A needs to have a higher liquid retention capacity than side B, and side B needs to have a higher adhesion force than side A. Smaller pore sizes result in higher adhesion force and lower liquid retention capacity. However, when the average pore size of side A is less than 1 μm or the average pore size of side B is less than 0.4 μm, the liquid retention capacity is too poor. Although the cell expansion rate is improved, lithium plating in the negative electrode area is more likely, and fast charging can easily lead to low battery cycle capacity retention, failing to effectively balance battery performance.

[0117] Furthermore, the polymer coating B of the diaphragms in Comparative Examples 2 and 6 had a lower average pore size of 0.3 μm, while the polymer coating M of the diaphragms in Comparative Examples 4 and 5 had a lower average pore size. A / M B The ratio is less than 0.5, and the M in the polymer coating of the diaphragm in Comparative Example 7 is... A / M B The ratio is greater than 3.5. If M A / M B If the ratio is less than 0.5, the adhesion of polymer coating B is too poor, leading to excessive cell expansion; if M A / M B A ratio greater than 3.5 indicates that although cell expansion is relatively small, the risk of lithium plating is relatively high, thus failing to effectively balance the battery's lithium plating and cell expansion performance.

[0118] In Example 2, the polymer coating A in the separator has a relatively large average pore size of 1.6 μm, and in Example 3, the polymer coating B in the separator has a relatively large average pore size of 1 μm. The larger particle size of the polymer coatings in Examples 2 and 3 results in insufficient adhesion of the coatings on either side A or B, leading to a larger cell expansion rate during charge-discharge cycles compared to Example 1. Therefore, the average pore size of the polymer coating A in the separator is preferably 1.3 μm, and the average pore size of the polymer coating B is preferably 0.7 μm. This can further improve the battery's capacity retention, cell expansion rate, and negative electrode lithium plating.

[0119] As shown in Table 3, compared to Example 1, the coating area of ​​the polymer coating on the separator in Example 6 is reduced, while the coating area of ​​the polymer coating on the separator in Example 7 is increased. It can be seen that the reduced coating area in Example 6 leads to decreased coating adhesion, causing the cell to expand slightly during charge-discharge cycles. Furthermore, the reduced coating area results in excessively large spacing between the strip-shaped polymer coatings, reducing the separator's electrolyte retention capacity and causing slight salt deposition in the negative electrode area. In Example 7, the increased coating area leads to a gradual decrease in the spacing between the strip-shaped polymer coatings, resulting in reduced electrolyte storage capacity and decreased electrolyte retention capacity of the cell. This makes the negative electrode area prone to slight lithium deposition, and the fast charging process may reduce the battery's cycle capacity retention rate. Therefore, the preferred coating areas for polymer coatings A and B are 70% and 80%, respectively. In Comparative Example 9, the separator polymer coating is fully coated, with no intermittent spaces on the separator surface to store electrolyte. The limited electrolyte storage capacity of the coating pores results in insufficient electrolyte retention capacity of the separator, leading to moderate lithium deposition during cycling. Comparative Examples 10-11 have a polymer coating on only one side of the separator, which cannot meet the battery's requirements for the separator's liquid retention capacity, nor can it effectively suppress the expansion of the cell, resulting in severe lithium plating during battery cycling and a high cell expansion rate.

[0120] As shown in Table 3, compared to Example 1, in Comparative Example 12, the coating strip in the separator is parallel to the length direction of the separator. In this case, the coating strip will result in low liquid injection efficiency of the cell during the liquid injection process, poor capillary action, and easy lithium deposition at the interface, resulting in poor performance. In Comparative Example 13, the coating strip in the separator is perpendicular to the length direction of the separator. The coating strip will easily cause lithium deposition in the corner area of ​​the cell, resulting in poor performance.

[0121] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit the scope of protection of this application. In particular, it should be noted that any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application for those skilled in the art.

Claims

1. A battery separator, characterized in that, The membrane substrate includes a surface A near the positive electrode and a surface B near the negative electrode. A polymer coating A is provided on surface A, and a polymer coating B is provided on surface B. The polymer coating A comprises at least two spaced-apart coating strips A, wherein the at least two coating strips A are distributed in parallel, and the ratio S of the area of ​​the polymer coating A to the area of ​​the surface A is... A It is 65%-70%; The polymer coating B comprises at least two spaced-apart coating strips B, wherein the at least two coating strips B are distributed in parallel, and the ratio S of the area of ​​the polymer coating B to the area of ​​the surface B is... B It is 75%-85%; One of the angles formed by the coating strip A and the length direction of the diaphragm substrate is an acute angle; one of the angles formed by the coating strip B and the length direction of the diaphragm substrate is an acute angle; Both polymer coating A and polymer coating B contain micropores, and the average pore size P of the micropores in polymer coating A is... A The micrometer size is 1.1-1.5 μm, and the pore size is (P... A -0.1) ~ (P A Pore ​​size distribution rate D (+0.1) μm A ≥80%; the average pore size P of the micropores contained in the polymer coating B B The micrometer size is 0.6-0.9 μm, and the pore size is (P B -0.1) ~ (P B Pore ​​size distribution rate D (+0.1) μm B ≥80%; The S A S B P A P B D A D B The following relationship exists between them: M A =S A ×P A ×D A M B = S B ×P B ×D B And 0.5≤M A / M B ≤3.

5.

2. The battery separator as described in claim 1, characterized in that, The polymer coating A is formed by coating and drying a polymer coating slurry A, wherein the polymer coating slurry A comprises solvent A1 and solvent A2 in a mass percentage ratio of (84-92):(8-16); The polymer coating B is formed by coating and drying a polymer coating slurry B, wherein the polymer coating slurry B comprises solvent B1 and solvent B2 in a mass percentage of (88-95):(5-12); Solvents A1 and B1 are each independently at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and acetone, and solvents A2 and B2 are each independently at least one of methanol, ethanol, isopropanol, n-butanol, and water.

3. A battery separator as described in claim 2, characterized in that, The polymer coating slurry A and polymer coating slurry B are each independent and also include a polymer with a mass fraction of 8wt%-15wt%.

4. The battery separator as described in claim 3, characterized in that, The polymers in polymer coating A and polymer coating B are each independent and include at least one of the following: polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trifluoroethylene copolymer, polyvinylidene fluoride-trifluorochloroethylene copolymer, polyvinylidene fluoride-tetrafluoroethylene copolymer, polyvinylidene fluoride-trifluoroethylene-trifluorochloroethylene copolymer, polyvinylidene fluoride-trifluoroethylene-chlorofluoroethylene copolymer, polyetherimide, polymethyl methacrylate, para-aramid, meta-aramid, and acrylate copolymer.

5. The battery separator as described in claim 1 or 2, characterized in that, The thicknesses of polymer coating A and polymer coating B are independent and range from 0.5 to 3 μm.

6. The battery separator as described in claim 1 or 2, characterized in that, The distance between two adjacent coating strips A is 0.2-3 mm, and one of the included angles formed between the coating strip A and the diaphragm substrate along the length direction is 30-60 degrees; And / or, the distance between two adjacent coating strips B is 0.2-3 mm, and one of the included angles formed between the coating strip B and the diaphragm substrate along the length direction is 30-60 degrees.

7. The battery separator as described in claim 1 or 2, characterized in that, The diaphragm substrate is at least one of polyethylene, polypropylene, polyethylene terephthalate, polyimide, aramid, and poly(terephthalic acid) butylene glycol. And / or, surface A and / or surface B of the diaphragm substrate are coated with at least one of the following: alumina, boehmite, magnesium oxide, magnesium hydroxide, barium titanate, aluminum hydroxide, silicon dioxide, aluminum nitride, lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide solid electrolyte, melamine cyanurate, melamine polyphosphate, ammonium polyphosphate, triphenyl phosphate, decabromodiphenyl ethane, tetrabromobisphenol A, brominated polystyrene, cellulose, and polyimide.

8. A method for preparing a battery separator as described in any one of claims 2-7, characterized in that, Includes the following steps: The polymer coating slurry A is coated on the surface A of the separator substrate, immersed in a coagulation bath and dried to form polymer coating A. The polymer coating slurry B is coated on the surface B of the separator substrate, immersed in a coagulation bath and dried to form polymer coating B, thus obtaining the battery separator.

9. A secondary battery, characterized in that, It includes a positive electrode, a negative electrode, an electrolyte, and a battery separator as described in any one of claims 1-7.

10. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 9.

Citation Information

Patent Citations

  • Separator for electrochemical device, having patterned electrode adhesive layer, and method for manufacturing separator

    CN112055899A