Acrylate monomer controllable free radical polymerization method based on organic tellurium compound
By using photo-induced in-situ generation of chain transfer agents from ditelluride compounds, the problems of long reaction cycles and limited molecular weight range in the TEP method were solved, enabling the efficient preparation of polyacrylate materials with molecular weights greater than 40,000, which has significant industrial application value.
Patent Information
- Application Number
- CN202510962788.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-11
- Publication Date
- 2025-11-28
AI Technical Summary
The traditional TEP method for preparing polyacrylate materials suffers from problems such as long reaction cycles, high energy consumption, numerous side reactions, and limited molecular weight range, making it difficult to meet the industrial application requirements of high-performance polymer materials.
A photoinduced ditelluride compound is used to generate a chain transfer agent in situ, which is then combined with an azobisisobutyronitrile initiator to carry out controlled free radical polymerization of acrylate monomers under light conditions at 40–80 °C. This simplifies the process and enables precise control of molecular weight and dispersion.
While reducing reaction temperature and cost, it increases polymerization efficiency by 7 to 20 times, enabling the preparation of ultra-high molecular weight polymers with molecular weights greater than 40,000, with well-defined chain-end structures that conform to the kinetic characteristics of controlled free radical polymerization.
Smart Images

Figure CN121021730A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer synthesis and preparation technology, and relates to a controlled free radical polymerization method for acrylate monomers based on organic ditellurium compounds. Background Technology
[0002] Polyacrylate polymers are a class of functional materials prepared from acrylate monomers through free radical polymerization. They possess characteristics such as tunable structure and diverse properties, and are widely used in adhesives, coatings, textiles, and pharmaceuticals. Due to their excellent biocompatibility, these materials also have significant application value in the medical field (such as drug carriers, medical dressings, and biosensors).
[0003] Traditional free radical polymerization methods struggle to precisely control the molecular weight and structure of polymers, while living radical polymerization (LRP) technology can achieve precise control over molecular weight (M... n ), Dispersion And precise control of end-group structures. Among them, organotellurium-regulated living radical polymerization (TERP) is a highly efficient and controllable synthetic method with the following advantages: Controllable molecular weight: By adjusting the ratio of monomer to chain transfer agent, the molecular weight of the polymer can be precisely designed. Narrow dispersion: The resulting polymer has a uniform molecular weight distribution and stable performance. Modifiable chain ends: The Te-C bonds at the polymer ends can be converted into active groups such as hydroxyl (-OH), amino (-NH2), and carboxyl (-COOH) through oxidation, click chemistry, etc., further expanding its functional applications.
[0004] Polyacrylate materials prepared based on the TEP method exhibit excellent performance in high-end adhesives (such as high-temperature pressure-sensitive adhesives), smart coatings (such as self-healing coatings), and biomedical materials (such as antibacterial catheter coatings), possessing significant industrial value and market prospects. In 2002, Yamago Shigeru et al. first reported the controlled free radical polymerization of styrene using organotelluric compounds as chain transfer agents (TERP method) (Yamago, S.; Iida, K.; Yoshida, J J Am. Chem. Soc. 2002, 124, 13666-13667.). The reaction formula is shown below. When the ratio of chain transfer agent to monomer is 1:100, the conversion rates of butyl acrylate and ethyl methacrylate monomers are 88% and 89%, respectively, after reacting at 100°C for 24 hours. However, this process suffers from long reaction cycles and high energy consumption, especially the stringent requirements for anhydrous and oxygen-free conditions, which have become the main bottleneck restricting the industrial application of the TEP method.
[0005]
[0006] In 2003, Yamago Shigeru et al. used AIBN initiator and an organic ditellurium compound to generate a chain transfer agent in situ at 100℃, and reacted it with butyl acrylate monomer for 24 hours, achieving a conversion rate of 88% and obtaining a polymer with controllable degree of polymerization and dispersion (Yamago, S.; Iida, K.; Nakajima, M.; Yoshida, J. Macromolecules 2003, 36, 3793-3796.). The reaction formula is shown below. This method has the following technical defects: 1) Defects in reaction conditions: High temperature (100℃) easily triggers side reactions such as chain end free radical bite-back, leading to a decrease in product purity; side reaction products will significantly affect the material properties of polymethyl acrylate (PMA); 2) Defects in kinetics: Excessive reaction time (24 hours) leads to an increase in the proportion of chain termination; the deactivation of active chains is aggravated, affecting the final polymer properties; 3) Molecular weight limitation: Only low molecular weight products (Mn≈7000) can be obtained, making it difficult to meet the requirements for the preparation of high molecular weight polymers. While this method simplifies the synthesis of chain transfer agents, the high temperatures and excessively long reaction times not only affect product purity but also severely limit the molecular weight range, making it difficult to meet the requirements for preparing high-performance polymer materials. These technical bottlenecks seriously restrict the industrial application prospects of this method.
[0007]
[0008] In 2013, Matsumoto Akikazu's research team achieved in-situ generation of an organic tellurium chain transfer agent at 60°C using a combination of diazo compounds and organic ditellurium compounds, and successfully applied it to the controlled free radical polymerization of polymethyl acrylate (PMA). The reaction formula is shown below. By precisely controlling the ratio of the two azo compounds, PMA polymers with a narrow molecular weight distribution (D<1.40) can be prepared. However, this technology has the following key technical defects: 1) Product structure defects: The use of a dual initiator system leads to complex and diverse end structures of polymer chains, making it difficult to accurately characterize the end-group structure of the product and seriously affecting the structure-activity relationship analysis of the product performance; 2) Process cost defects: The key catalyst V-70 has stability issues: it is prone to spontaneous decomposition at room temperature and requires low-temperature storage (below -10°C), and the catalyst is expensive, significantly increasing production costs; 3) Polymerization mechanism defects: The actual polymerization kinetics deviate from the ideal controlled polymerization characteristics, does not conform to the first-order kinetic equation, and the initiation efficiency deviates significantly from the theoretical value. Although this system has made progress in controlling reaction temperature and regulating dispersion, its application in industrial production is severely limited by the aforementioned technical shortcomings, particularly the uncontrollable product structure and catalyst stability issues. These fundamental problems urgently need to be addressed through the design of new catalytic systems.
[0009] Summary of the Invention
[0010] This invention addresses the technical problem of uncontrollable molecular weight and structure of polyacrylates in organotelluric acid-regulated living radical polymerization (TERP) reactions. It provides a controllable free radical polymerization method for acrylate monomers based on organoditelluric acid compounds. The method uses photo-induced ditelluric acid ether compounds to generate chain transfer agents in situ. By simultaneously controlling the molecular weight and dispersion, ultra-high molecular weight polymer products with a molecular weight greater than 40,000 can be obtained.
[0011] To achieve the above objectives, the present invention adopts the following technical solution:
[0012] This invention provides a controlled free radical polymerization method for acrylate monomers based on organic ditellurium compounds, comprising the following steps:
[0013] Using azobisisobutyronitrile as an initiator and diphenyl ditelluride as a chain transfer agent, free radical polymerization of acrylate monomers was carried out under an inert gas atmosphere and light irradiation to obtain polyacrylate compounds with controllable molecular weight and dispersion; the reaction formula is as follows:
[0014]
[0015] Where: R stands for -COO(CH3) m m = 1 to 4.
[0016] In the above technical solution, the reaction temperature is 40-80℃ and the reaction time is 1-3h.
[0017] In the above technical solution, the molar ratio of the acrylate monomer, azobisisoheptanenitrile, and diphenylditelluride compound is 30-1000:0.4-1:1.
[0018] In the above technical solution, the inert gas atmosphere is a nitrogen or argon atmosphere.
[0019] In the above technical solution, the wavelength of the illumination condition is not less than 420nm.
[0020] In the above technical solution, the acrylate monomers are selected from methyl acrylate, ethyl acrylate, n-butyl acrylate or isobutyl acrylate.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0022] Raw material advantages: Using industrial-grade conventional raw materials, compared with the dual-initiator system of azo compounds, it avoids the use of expensive and unstable special catalysts, significantly reducing material costs.
[0023] Process innovation: For the TERP system, a photo-induced in-situ generation technology of ditelluride compounds to generate chain transfer agents is adopted to achieve true "one-pot" continuous polymerization without the need for pre-synthesis and purification of chain transfer agents.
[0024] Production benefits: Using a single azo compound as the initiator system simplifies the process. Compared with a single initiator system that requires heating, the polymerization efficiency is increased by 7 to 20 times while reducing the reaction temperature by 20°C.
[0025] Product performance: This invention can obtain ultra-high molecular weight polymer products with a molecular weight greater than 40,000 while simultaneously controlling molecular weight and dispersion. Furthermore, due to the single initiator system, the chain end structure of the polymer is well-defined.
[0026] This invention achieves synergistic control of photoinduced in-situ synthesis and polymerization, overcoming the process limitations of the traditional TEP method and providing a practical technical solution for industrial production. This method is not only simple to operate, but also exhibits significant advantages in product quality, production cost, and process stability, making it of significant industrial application value. Attached Figure Description
[0027] Figure 1 This is a graph showing the relationship between the conversion rate of the monomer in Example 1 and time.
[0028] Figure 2 The kinetic equation for the conversion rate of the monomer in Example 1 versus time is shown.
[0029] Figure 3 The graph shows the relationship between the conversion rate of the monomer in Example 1 and its molecular weight and dispersibility.
[0030] Figure 4 The graph shows the conversion rate versus molecular weight GPC of the monomer in Example 1.
[0031] Figure 5 This is a graph showing the relationship between the conversion rate of the monomer in Example 6 and time.
[0032] Figure 6 The kinetic equation for the conversion rate versus time of the monomer in Example 6 is shown.
[0033] Figure 7 The graph shows the relationship between the conversion rate of the monomer in Example 6 and its molecular weight and dispersibility.
[0034] Figure 8 The graph shows the conversion rate versus molecular weight GPC of the monomer in Example 6.
[0035] Figure 9 The graph shows the relationship between the conversion rate of the monomer in Example 9 and time.
[0036] Figure 10The kinetic equation for the conversion rate versus time of the monomer in Example 9 is shown.
[0037] Figure 11 The graph shows the relationship between the conversion rate of the monomer in Example 9 and its molecular weight and dispersibility.
[0038] Figure 12 The graph shows the conversion rate versus molecular weight GPC of the monomer in Example 9. Detailed Implementation
[0039] The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the test methods in the following embodiments are conventional methods.
[0040] The monomer raw materials methyl acrylate (MA), n-butyl acrylate (BA), and isobutyl acrylate (i-BA) used in the following examples all required neutral alumina column treatment before use. Diphenyl ditelluride (DHDT) and other reagents were commercially available and ready for direct use.
[0041] In the following examples, the structural characterization of the synthesized compounds and the monomer conversion during polymerization were obtained by nuclear magnetic resonance (NMR, Bruker 400MHz). The number-average molecular weight (Mn) of the synthesized polymers was... n ) and its dispersion value This was achieved using a TOSOH-HLC-8320 gel permeation chromatography (GPC) system equipped with a refractive index detector. The chromatograph used a TSK Gel Super AWM-H column (4.6 mm ID × 15 cm × 2), which has a wide molecular weight measurement range from 10... 3 Up to 10×10 5 g mol -1 The test must be conducted at 40°C, using THF or DMF as the eluent, with a flow rate controlled at 0.5 mL / min. -1 Samples were introduced using a TOSOH autosampler, and PMMA or PS standard samples were used as calibration standards during data analysis.
[0042] Comparative Example 1: Preparation of polymethyl acrylate with a degree of polymerization of 100 under heating conditions
[0043] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (14 mg, 0.049 mmol), and MA (420 mg, 4.9 mmol) was stirred in an oil bath at 80 °C for 24 h. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved a 90% monomer conversion, and 374 mg of polymethyl acrylate (91% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The value is 7200, and the dispersion (D) is 1.19.
[0044] Example 1: Preparation of polymethyl acrylate with a degree of polymerization of 100 under heating and light irradiation conditions.
[0045] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and MA (422 mg, 4.9 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 2 h to remove wavelengths below 420 nm. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved a monomer conversion of 97%, and 384 mg of polymethyl acrylate (PMMA) was obtained by vacuum distillation (94% yield). The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The concentration was 7900, the dispersion (D) was 1.20, and chain extension experiments confirmed that the end-group fidelity reached 92%. Furthermore, the polymerization process conformed to the kinetic characteristics of controlled radical polymerization. Figure 1-4 As shown.
[0046] Compared with Comparative Example 1, this embodiment improved monomer conversion, number-average molecular weight, and dispersion by increasing light conditions.
[0047] Example 2: Preparation of polymethyl acrylate with a degree of polymerization of 100 under different heating temperatures and light irradiation conditions.
[0048] Under nitrogen protection, chain transfer agent diphenyl ditelluride (DHDT) (20 mg, 0.049 mmol), initiator azobisisobutyronitrile (V65) (12 mg, 0.049 mmol), and methyl acrylate monomer (MA) (422 mg, 4.9 mmol) were mixed and stirred at different temperatures. The reaction was then filtered to remove mercury lamp irradiation at wavelengths below 420 nm or 470 nm. Nuclear magnetic resonance (NMR) was used to analyze the reaction. 1 The reaction process was monitored in real time and the product characteristics were analyzed using 1H NMR and gel permeation chromatography (GPC). The results are shown in Table 1. It can be seen that when the wavelength is greater than 470 nm, the monomer conversion rate is very low after 24 h of reaction. However, when 420 nm is used, the monomer conversion rate and molecular weight gradually increase with the increase of reaction temperature and the shortening of reaction time. Therefore, the wavelength of light irradiation needs to be greater than 420 nm.
[0049]
[0050] Table 1. Experimental results under different experimental temperatures and light conditions.
[0051]
[0052] Example 3: Preparation of polymethyl acrylate with a degree of polymerization of 100 under different molar ratios, heating, and light irradiation conditions.
[0053] Under nitrogen protection, chain transfer agent DHDT (20 mg, 0.049 mmol), initiator V65 (5–18 mg, 0.019–0.072 mmol), and MA (422 mg, 4.9 mmol) were mixed and irradiated with mercury lamps at a constant temperature of 80 °C with stirring. The reaction was monitored by filtering out wavelengths below 420 nm using a mercury lamp irradiation method. The reaction progress was recorded by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The results are shown in Table 2. It can be seen that the monomer conversion and dispersibility were highest when the V65:DHDT molar ratio was 0.4:1.
[0054] Table 2 Experimental results of DHDT and V65 at different molar ratios
[0055]
[0056]
[0057] Example 4: Preparation of polymethyl acrylate with a degree of polymerization of 300 under heating and light irradiation conditions.
[0058] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and MA (1.3 g, 14.7 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 3 h to remove wavelengths below 420 nm using a filter. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction yielded a monomer conversion of 87%, and 1.04 g of polymethyl acrylate (92% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The value is 20600, and the dispersion (D) is 1.34.
[0059] Example 5: Preparation of polymethyl acrylate with a degree of polymerization of 500 under heating and light irradiation conditions.
[0060] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and MA (2.1 g, 24.5 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 4 h, with wavelengths below 420 nm filtered out. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved an 85% monomer conversion, and 1.99 g of polymethyl acrylate (89% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The value is 33200, and the dispersion (D) is 1.42.
[0061] Example 6: Preparation of polybutyl acrylate with a degree of polymerization of 100 under heating and light irradiation conditions.
[0062] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and BA (0.6 g, 4.9 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 2 h to remove wavelengths below 420 nm using a filter. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction yielded an 85% monomer conversion, and 595 mg of polymethyl acrylate (89% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The polymerization coefficient (D) is 10600, the dispersion (D) is 1.22, and the end-group fidelity is 90%. The polymerization process conforms to the kinetic characteristics of controlled radical polymerization, such as... Figure 5-8 As shown.
[0063] Example 7: Preparation of polybutyl acrylate with a degree of polymerization of 300 under heating and light irradiation conditions.
[0064] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and BA (1.88 g, 14.7 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 3 h to remove wavelengths below 420 nm. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved an 85% monomer conversion, and 1.8 g of polymethyl acrylate (92% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The value is 25000, and the dispersion (D) is 1.35.
[0065] Example 8: Preparation of polybutyl acrylate with a degree of polymerization of 500 under heating and light irradiation conditions.
[0066] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and BA (3.14 g, 24.5 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 3 h to remove wavelengths below 420 nm using a filter. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved a 90% monomer conversion, and 2.44 g of polymethyl acrylate (91% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The value is 43200, and the dispersion (D) is 1.47.
[0067] Example 9: Preparation of polyisobutyl acrylate with a degree of polymerization of 100 under heating and light irradiation conditions.
[0068] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and i-BA (0.6 g, 4.9 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 2 h to remove wavelengths below 420 nm using a filter. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved a 90% monomer conversion, and 496 mg of polymethyl acrylate (89% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The polymerization coefficient was 9800, the dispersion (D) was 1.21, and the end-group fidelity was 90%. Furthermore, the polymerization process conformed to the kinetic characteristics of controlled radical polymerization, such as... Figure 9-12 As shown.
[0069] Example 10: Preparation of polybutyl acrylate with a degree of polymerization of 300 under heating and light irradiation conditions.
[0070] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and i-BA (1.88 g, 14.7 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 3 h to remove wavelengths below 420 nm using a filter. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved a 90% monomer conversion, and 1.59 g of polymethyl acrylate (92% yield) was obtained by vacuum distillation. The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value].n The value is 23800, and the dispersion (D) is 1.28.
[0071] Example 11: Preparation of polybutyl acrylate with a degree of polymerization of 500 under heating and light irradiation conditions.
[0072] Under nitrogen protection, a mixed solution of DHDT (20 mg, 0.049 mmol), V65 (12 mg, 0.049 mmol), and i-BA (3.14 g, 24.5 mmol) was stirred in an oil bath at 80 °C while the reaction was irradiated with a mercury lamp for 4 h, with wavelengths below 420 nm filtered out. The reaction progress was monitored by proton nuclear magnetic resonance spectroscopy (1H NMR). 1 Real-time monitoring and product characterization were performed using 1H NMR and gel permeation chromatography (GPC). The reaction achieved a monomer conversion of 92%, and 1.59 g of polymethyl acrylate (PMMA) was obtained by vacuum distillation (92% yield). The product was analyzed by SEC, showing a number-average molecular weight (Mn) of [missing value]. n The value is 40200, and the dispersion (D) is 1.49.
[0073] The embodiments described above are merely preferred embodiments of the present invention and are only used to explain the present invention. They are not intended to limit the scope of the present invention. For those skilled in the art, other implementation methods can be easily made by substitution or modification based on the technical content disclosed in this specification. Therefore, all changes and improvements made on the principle of the present invention should be included within the scope of the patent application of the present invention.
Claims
1. A controlled radical polymerization process of acrylate-based monomers based on organic ditellurium compounds, characterized in that, The method comprises the following steps: The free radical polymerization of the acrylic ester monomer is carried out in an inert gas atmosphere under light conditions, with azobisisoheptane nitrile as an initiator and diphenyl ditelluride as a chain transfer agent, to obtain a polyacrylic ester compound with controllable molecular weight and dispersity; the reaction formula is as follows: wherein: R is -COO(CH3) m m = 1-4.
2. The controlled radical polymerization method of an acrylate-based monomer based on an organic ditellurium compound according to claim 1, characterized by, The reaction temperature is 40-80℃, and the reaction time is 1-3h.
3. The method according to claim 1, wherein the organic ditellurium compound is represented by the following formula (1) : ###0001### (1) wherein R1 to R4 each independently represent a hydrogen atom or a hydrocarbon group, and R5 and R6 each independently represent a hydrocarbon group, provided that at least one of R5 and R6 is a hydrocarbon group having 1 or more carbon atoms. The molar ratio of the acrylic ester monomer, azobisisoheptane nitrile and diphenyl ditelluride compound is 30-1000:0.4-1:
1.
4. The controlled radical polymerization method of an acrylate-based monomer using an organic ditellurium compound according to claim 1, characterized by, The inert gas atmosphere is a nitrogen or argon atmosphere.
5. The controlled free radical polymerization method for acrylate monomers based on organic ditellurium compounds according to claim 1, characterized in that, The wavelength of the light condition is not less than 420nm.