Battery separator and its preparation method, secondary battery

By modifying the surface of the microporous membrane and applying a coating, the problem of improving the performance of existing polyolefin microporous membranes without sacrificing the pore-closing temperature was solved, resulting in increased membrane rupture temperature and tensile strength, thus enhancing the safety and stability of the battery.

CN121642437BActive Publication Date: 2026-11-17SINOMA LITHIUM BATTERY SEPARATOR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511623388.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-11-06
Publication Date
2026-11-17
Estimated Expiration
2045-11-06

AI Technical Summary

Technical Problem

Existing polyolefin microporous membranes cannot simultaneously improve rupture temperature, tensile strength, and puncture strength without sacrificing pore-closing temperature.

Method used

Modified microporous membranes are prepared by modifying the surface of microporous membranes with aromatic compounds containing alkenyl and ester groups, combined with ultraviolet irradiation and surface irradiation techniques, and then coating one or both sides of the membrane with a coating to improve the membrane's performance.

Benefits of technology

Without affecting the pore closure temperature, the rupture temperature, tensile strength, puncture resistance and conductivity of the microporous membrane were significantly improved, thereby enhancing the safety and stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_7
    Figure SMS_7
  • Figure SMS_8
    Figure SMS_8
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

This invention discloses a battery separator, its preparation method, and a battery. The battery separator comprises a microporous membrane and a coating. The microporous membrane is obtained by surface modification with aromatic compounds containing alkenyl and ester groups. This invention, by grafting aromatic compounds containing alkenyl and ester groups onto the surface of the microporous membrane, suppresses side reactions between the electrolyte solvent and the positive and negative electrode plates, thereby improving the cycle stability of the battery. Furthermore, the preparation method of surface irradiation followed by crosslinking modification of the microporous membrane improves its puncture resistance, membrane rupture temperature, tensile strength, and conductivity without significantly affecting its pore-closure temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery separator technology, specifically relating to a battery separator and its preparation method, and a secondary battery. Background Technology

[0002] Battery separators are thin films with microporous structures that separate the positive and negative electrodes. They are one of the key materials with the greatest technological barriers in the secondary battery industry chain. They mainly serve two functions: separating the positive and negative electrodes to prevent short circuits and providing microchannels to support ion migration. They directly affect the battery's safety performance, cycle life, and other characteristics.

[0003] Polyolefin microporous membranes have good stability and low cost, and are currently the most commercially mature membrane products. The main base materials include polyethylene (PE) and polypropylene (PP). The mainstream products are single-layer PP microporous membranes, single-layer PE microporous membranes, and three-layer PP / PE / PP microporous composite membranes. However, polyolefin microporous membranes still have many defects such as low porosity and poor affinity for electrolytes.

[0004] Patent CN 114094284A discloses a novel cross-linked separator and its preparation method. It uses acrylates containing multiple branches as monomers to cross-link PE, improving its rupture temperature, tensile strength, and puncture strength. However, this also significantly increases the overall pore-closing temperature of the separator, affecting battery safety. Currently, obtaining a separator that improves rupture temperature, tensile strength, and puncture strength without sacrificing pore-closing temperature is a pressing problem in this field. Summary of the Invention

[0005] The purpose of this invention is to provide a battery separator that solves the problem that existing separators cannot increase the rupture temperature while keeping the pore-closing temperature constant or even decreasing it.

[0006] Another object of the present invention is to provide a method for preparing a battery separator.

[0007] Another object of the present invention is a secondary battery.

[0008] In a first aspect, the present invention provides a battery separator comprising a microporous membrane and a coating, wherein the microporous membrane is obtained by surface modification with an aromatic compound containing alkenyl and ester groups.

[0009] Secondly, the present invention provides a method for preparing a battery separator, comprising the following steps:

[0010] I. Preparation of modified microporous membranes:

[0011] S1, Dissolve aromatic compounds containing alkenyl and ester groups in a solvent, add an initiator, and prepare a modified solution;

[0012] S2, the microporous membrane material is surface treated after being melt-cast, biaxially stretched, extracted and dried to generate free radicals on the surface of the microporous membrane. The modified solution is then brought into contact with the surface-treated microporous membrane, and then subjected to ultraviolet irradiation. After curing, it is cleaned, dried and subjected to secondary transverse stretching to obtain the modified microporous membrane.

[0013] II. Coating Preparation:

[0014] Step A: Prepare the coating slurry;

[0015] Step B involves applying a coating slurry to at least one side of the modified microporous membrane.

[0016] The present invention also provides another method for preparing a battery separator, comprising the following steps:

[0017] Step A': Prepare the coating slurry;

[0018] Step B': Apply the coating slurry to at least one side of the finished microporous membrane and dry it;

[0019] Step C' involves dissolving aromatic compounds containing alkenyl and ester groups in a solvent, then adding an initiator to prepare a modified solution;

[0020] Step D' involves surface-treating the microporous membrane coated in step B' to generate free radicals on the surface of the microporous membrane. The modified solution is then brought into contact with the surface-treated membrane, followed by ultraviolet irradiation. After curing, the membrane is cleaned and dried to obtain the modified diaphragm.

[0021] Thirdly, the present invention provides a secondary battery including the above-described battery separator.

[0022] Beneficial effects of this invention:

[0023] This invention achieves the suppression of side reactions between the electrolyte solvent and the positive and negative electrode plates and improves the cycle stability of the battery by grafting aromatic compounds containing alkenyl and ester groups onto the surface of a microporous membrane. Moreover, by using a preparation method of surface irradiation followed by crosslinking modification of the microporous membrane, its puncture resistance, membrane rupture temperature, tensile strength, and conductivity are improved with minimal impact on its pore closure temperature. Detailed Implementation

[0024] The present invention will now be described in detail through embodiments. It should be noted that the following embodiments are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above description.

[0025] The present invention provides a battery separator, comprising a microporous membrane and a coating, wherein the microporous membrane is obtained by surface modification with an aromatic compound containing alkenyl and ester groups.

[0026] In the battery separator of the present invention, the aromatic compound containing alkenyl and ester groups is one or more of the compounds shown in Formulas I-1 to I-6.

[0027] Formula I-1;

[0028] Formula I-2;

[0029] Formula I-3;

[0030] Formula I-4;

[0031] Formula I-5;

[0032] Formula I-6.

[0033] In the battery separator of the present invention, the microporous membrane may be a polyethylene membrane, polypropylene membrane, polyimide membrane, aramid membrane or aramid sulfone membrane modified with an aromatic compound containing alkenyl and ester groups.

[0034] The present invention also provides a method for preparing the battery separator, comprising the following steps:

[0035] I. Preparation of modified microporous membranes:

[0036] S1, Dissolve aromatic compounds containing alkenyl and ester groups in a solvent, add an initiator, and prepare a modified solution;

[0037] S2, the microporous membrane obtained by melting and casting, biaxial stretching, extraction and drying is subjected to surface treatment to generate free radicals on the surface of the microporous membrane. The modified solution is then brought into contact with the surface-treated microporous membrane, followed by ultraviolet irradiation, curing, cleaning, drying and secondary transverse stretching to obtain the modified microporous membrane.

[0038] II. Coating Preparation:

[0039] Step A: Prepare the coating slurry;

[0040] Step B involves applying a coating slurry to at least one side of the modified microporous membrane.

[0041] Step S2 of this preparation method involves the conventional preparation methods in the art, including melt casting, biaxial stretching, extraction and drying, and secondary transverse stretching of the microporous membrane. Specific preparation conditions are not limited. The characteristic of this invention is that after extraction and drying and before secondary transverse stretching, it further includes surface treatment of the microporous membrane, contact with a modification solution, and UV curing to complete the modification of the microporous membrane. The biaxial stretching can be synchronous or asynchronous.

[0042] The method for preparing the battery separator of the present invention uses an aromatic compound containing olefinic and ester groups, which accounts for 0.2% to 20% of the mass of the modified microporous membrane. Specifically, the amount can be 0.2%, 0.5%, 1%, %, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%. This value is calculated using the formula: (mass of the modified microporous membrane - mass of the unmodified microporous membrane) / mass of the modified microporous membrane.

[0043] In the preparation method of the battery separator described in this invention, surface treatment is performed in step S2 by surface irradiation or photodegradation. In this invention, the purpose of surface irradiation and photodegradation is to generate free radicals on the surface of the microporous membrane. The specific methods and conditions for surface irradiation and photodegradation are not specifically limited in this invention, as long as they can generate free radicals on the microporous membrane surface. Preferably, surface irradiation involves irradiating the separator surface with a cobalt source or an electron accelerator at an irradiation dose of 0.1–1 mgy, specifically 0.1 mgy, 0.2 mgy, 0.3 mgy, 0.4 mgy, 0.5 mgy, 0.6 mgy, 0.7 mgy, 0.8 mgy, 0.9 mgy, or 1 mgy, where free radicals are generated on the surface under the action of high-energy rays. Photodegradation refers to irradiating the surface with ultraviolet light (wavelength below 450 nm) to generate free radicals.

[0044] In the preparation method of the battery separator of the present invention, during the curing in step S2, the ultraviolet irradiation conditions are as follows: the ultraviolet wavelength is 200~450nm, specifically 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, and the time is ≤60s, specifically 5s, 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s.

[0045] In the preparation method of the battery separator of the present invention, the content of aromatic compounds containing alkenyl and ester groups in the modified solution of step S1 is 2~40 wt%, specifically 2 wt%, 3 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, and 40 wt%.

[0046] The battery separator preparation method of the present invention, wherein the modified solution in step S1 contains 3-25 wt% aromatic compounds with alkenyl and ester groups, and the separator has high tensile strength, with a transverse tensile strength reaching 2076-2302 kgf / cm². 2 The longitudinal tensile strength can reach 2263~2513 kgf / cm. 2 It exhibits low thermal shrinkage, with transverse thermal shrinkage reaching 0.4~1.6% and longitudinal thermal shrinkage reaching 0.8~2.7%; electrical conductivity reaching 6.9~8.0 mS / cm; puncture strength reaching 351~675gf; pore-closing temperature as low as 136.7~142.6℃; and membrane rupture temperature as high as 172.2~223.9℃.

[0047] The method for preparing the battery separator according to the present invention uses an initiator that is at least one selected from benzoin ethers, α-hydroxy ketones, acetophenone derivatives, acylphosphine oxides, benzophenone, thioxanthones, and anthraquinones, preferably acylphosphine oxides.

[0048] In the preparation method of the battery separator of the present invention, the acylphosphine oxide can be TPO (2,4,6-trimethylbenzoyl diphenylphosphine oxide), TMO (2,4,6-trimethylbenzoyl di(p-tolyl)phosphine oxide), BAPO (phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide), or TPO-L (ethyl(2,4,6-trimethylbenzoyl)phenylphosphine ester).

[0049] In the method for preparing the modified microporous membrane of the present invention, the amount of initiator added is 1 to 15 wt% of the amount of the aromatic compound containing alkenyl and ester groups added (for example, it can be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, or 15 wt%).

[0050] The method for preparing the modified microporous membrane according to the present invention uses a solvent that is at least one of ethers, esters, and haloalkanes.

[0051] The method for preparing the modified microporous membrane of the present invention uses a solvent that is at least one selected from methyl ethyl carbonate, dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, acetone, and DMAc.

[0052] This invention also provides another method for preparing a battery separator, comprising the following steps:

[0053] Step A': Prepare the coating slurry;

[0054] Step B': Apply the coating slurry to at least one side of the finished microporous membrane and dry it;

[0055] Step C' involves dissolving an aromatic compound containing alkenyl and ester groups in a solvent, then adding an initiator to prepare a modified solution;

[0056] Step D' involves surface-treating the membrane coated in step B' to generate free radicals on the surface of the microporous membrane. The modified solution is then brought into contact with the surface-treated microporous membrane, followed by ultraviolet irradiation. After curing, the membrane is cleaned and dried to obtain the modified diaphragm.

[0057] In this preparation method, the finished microporous membrane is obtained by purchasing or by conventional methods in the art. The difference between this and the aforementioned modified microporous membrane is that the finished microporous membrane is a microporous membrane that has undergone secondary transverse stretching.

[0058] In the above two methods for preparing battery separators, the specific preparation method and raw material composition of the coating slurry are not specifically limited by this invention, as they are conventional techniques in the field. Those skilled in the art can adjust and select according to actual needs. The coating slurry may contain inorganic substances and / or high-temperature resistant organic polymers, water or organic solvents, and may also contain binders, wetting agents, etc. When modifying the surface of the microporous membrane, modification can be performed on one side or both sides.

[0059] The modified solution used in step C' can be the same as the modified solution used in step S1 of the aforementioned method, that is, the content of aromatic compounds containing alkenyl and ester groups in the modified solution is 2 to 40 wt%, specifically 2 wt%, 3 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, or 40 wt%. The amount and type of initiator can also be the same as the initiator used in step S1 of the aforementioned method, that is, the initiator can be at least one of benzoin ethers, α-hydroxy ketones, acetophenone derivatives, acylphosphine oxides, benzophenone, thioxanthones, and anthraquinones, preferably acylphosphine oxides, and the amount added is 1 to 15 wt% of the amount of the aromatic compounds containing alkenyl and ester groups added (for example, it can be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, or 15 wt%).

[0060] The surface treatment and curing methods and conditions for the coated film in step D' are the same as those for the aforementioned preparation method, namely, surface treatment is performed by surface irradiation or photodegradation. The purpose of surface irradiation and photodegradation is to generate free radicals on the surface of the microporous membrane. The specific methods and conditions for surface irradiation and photodegradation are not specifically limited in this invention, as long as they can generate free radicals on the microporous membrane surface. Preferably, surface irradiation involves irradiating the membrane surface with a cobalt source or an electron accelerator at a dose of 0.1–1 mgy, specifically 0.1 mgy, 0.2 mgy, 0.3 mgy, 0.4 mgy, 0.5 mgy, 0.6 mgy, 0.7 mgy, 0.8 mgy, 0.9 mgy, or 1 mgy. Free radicals are generated on the microporous membrane surface under the action of high-energy rays. Photodegradation refers to irradiating the surface with ultraviolet light (wavelength below 450 nm) to generate free radicals. During curing, the ultraviolet irradiation conditions are: ultraviolet wavelength of 200–450 nm, specifically 200 nm, 250 nm, 300 nm, 350 nm, or 400 nm. nm, 450nm, time ≤60s, specifically can be 5s, 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s.

[0061] When coating a microporous membrane, the coating can be applied to one side of the microporous membrane or to both sides of the microporous membrane. The coating method is a conventional technique in the field, and the present invention does not impose specific limitations. Those skilled in the art can choose according to actual needs.

[0062] In the two battery separator preparation methods mentioned above, the coating thickness on the microporous membrane surface, that is, the coating thickness on the modified microporous membrane surface or the coating thickness on the finished microporous membrane surface, can be 0.5μm~6μm, specifically 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, and 6μm.

[0063] The method of the present invention will be described in detail below through specific embodiments.

[0064] Example 1

[0065] (1) The compound shown in Formula I-2 was dissolved in ethyl methyl carbonate, and then an acylphosphine oxide (TPO) initiator was added to prepare a modified solution with a compound content of 3 wt% and the amount of initiator was 5 wt% of the compound shown in Formula I-2;

[0066] (2) Polyethylene with a viscosity-average molecular weight of 1 million and white oil were melted, mixed and extruded to form a casting sheet, and then subjected to simultaneous biaxial stretching (the stretching ratio of longitudinal stretching and transverse stretching was 6 times, and the temperature was 120℃), extraction and drying to obtain a PE microporous membrane. The membrane was then irradiated on both sides with a cobalt source (irradiation dose 1 MGy).

[0067] (3) The above-mentioned surface-treated membrane was immersed in the modified solution, and then irradiated with ultraviolet light with a wavelength of 380 nm for 60 s. After cleaning, drying and secondary stretching (stretch ratio 1.1 times, 130℃), a modified microporous membrane with a thickness of 9 μm was obtained.

[0068] (4) Alumina (D50 is 500nm), binder (carboxymethyl cellulose and polyacrylate 1:2) and dispersant (polyacrylic acid) with a mass ratio of 94:6:0.5 are dissolved in water to prepare a coating slurry with a solid content of 36%. The coating slurry is coated on both sides of the modified microporous membrane in step (3) with a coating thickness of 2μm to obtain the battery separator.

[0069] Examples 2-4

[0070] The preparation method is the same as in Example 1, except that the mass content of the compound shown in Formula I-2 in the modified solution in step (1) is different. Please see Table 1 for details.

[0071] Examples 5-8

[0072] The preparation method is the same as in Example 3, except that the aromatic compounds in step (1) are different, as detailed in Table 1.

[0073] Example 9

[0074] (1) The compound shown in Formula I-2 was dissolved in methyl ethyl carbonate, and then an acylphosphine oxide (TPO) initiator was added to prepare a modified solution with a compound content of 15 wt%, wherein the amount of initiator was 5 wt% of the compound shown in Formula I-2;

[0075] (2) Alumina (D50 is 500nm), binder (carboxymethyl cellulose and polyacrylate 1:2) in a mass ratio of 94:6:0.5, and dispersant (polyacrylic acid) are dissolved in water to prepare a coating slurry with a solid content of 36%. The coating slurry is coated on both sides of a finished PE microporous membrane (Sinoma Lithium Membrane Co., Ltd., SNP9) with a thickness of 9μm. The coating thickness is 2μm to obtain a membrane with coating.

[0076] (3) The coated diaphragm prepared in step (2) was irradiated on both sides with a cobalt source (irradiation dose 1 mgy).

[0077] (4) The surface-treated coated separator is immersed in the modified solution prepared in step (1), and then irradiated with ultraviolet light with a wavelength of 380nm for 60s. After cleaning and drying, the battery separator is obtained.

[0078] Example 10

[0079] The preparation method is the same as in Example 9, except that the aromatic compound in step (1) is the compound shown in Formula I-3, and the microporous membrane is the finished PE microporous membrane (SNP9) from Sinoma Lithium Membrane Co., Ltd.

[0080] Example 11

[0081] The preparation method is the same as in Example 9, except that the aromatic compound in step (1) is the compound shown in Formula I-1.

[0082] Comparative Example 1

[0083] (1) Polyethylene with a viscosity-average molecular weight of 1 million and white oil were melted, mixed and extruded to form a cast sheet, and then subjected to simultaneous biaxial stretching (stretching ratio of 6 times for longitudinal stretching and transverse stretching, temperature of 120℃), extraction, drying and secondary transverse stretching (stretching ratio of 1.1 times, 130℃) to obtain a PE microporous membrane with a thickness of 9μm.

[0084] (2) Alumina (D50 is 500nm), binder (carboxymethyl cellulose and polyacrylate 1:2) and dispersant (polyacrylic acid) with a mass ratio of 94:6:0.5 are dissolved in water to prepare a coating slurry with a solid content of 36%. The coating slurry is coated on both sides of the microporous membrane in step (3) with a coating thickness of 2μm to obtain the battery separator.

[0085] Comparative Example 2

[0086] The preparation method is the same as in Example 3, except that the modified material in step (1) is different. Please see Table 1 for details.

[0087] The battery separators prepared in the examples and comparative examples were subjected to the following performance tests.

[0088] Compound content in modified microporous membrane / modified diaphragm: In Examples 1-8 and Comparative Example 2, the method for testing the compound content in the modified microporous membrane is as follows: cut a 1m*1m microporous membrane sample obtained in step (2), measure its mass and record it as m1, cut a 1m*1m microporous membrane sample after drying in step (3) and before the second horizontal stretching, measure its mass and record it as m2, take 5 groups of samples, take their average value, and then the compound content in the modified microporous membrane is (m2-m1) / m2*100%.

[0089] In Examples 9-11, the method for testing the compound content in the modified diaphragm is as follows: cut a 1m*1m diaphragm sample obtained in step (3), measure its mass and record it as m1, cut a 1m*1m diaphragm sample from step (4), measure its mass and record it as m2, take 5 groups of samples, and take their average value. Then the compound content in the modified diaphragm is (m2-m1) / m2*100%.

[0090] Puncture resistance:

[0091] The test was conducted according to the method specified in GB / T 36363-2018. A diaphragm with a size of 50*100 mm was cut along the TD direction. The diaphragm was fixed on the sample fixture of the puncture test machine (model: KES-GNDG5, KNC Technology Co., Ltd.). A steel needle with a diameter of 1.0 mm was used to puncture the diaphragm at a speed of 0.1 cm / sec. The maximum load of the steel needle penetrating the diaphragm was read. The test was performed more than 5 times and the arithmetic mean was taken.

[0092] Electrical conductivity:

[0093] Assemble an Al|separator|Al symmetric cell, inject electrolyte (EC / DMC = 3:7, LiPF6 1M), and vacuum seal. Connect the test circuit and apply an AC signal using an electrochemical workstation or similar instrument; the frequency range is typically from 10 mHz to 100 kHz. Record impedance data at different frequencies and plot the impedance spectrum. Fit and analyze the impedance spectrum using an equivalent circuit model to obtain the membrane resistance value.

[0094] The conductivity is calculated using the formula σ=L / RS, where σ is the conductivity, L is the membrane thickness, R is the membrane resistance, and S is the contact area between the electrode and the membrane.

[0095] Tensile strength:

[0096] The test was conducted according to GB / T 1040.3-2006. Under the test requirements of 23±3℃ and ≤60% humidity, a 1.5cm×20cm sample was cut and marked with the MD / TD direction of the diaphragm. The sample was tested using a tensile testing machine (High-Speed ​​Rail Testing Instruments (Dongguan) Co., Ltd., AI-3000-SU). The sample was fixed between the upper and lower clamps of the tensile testing machine (the distance between the clamps was 100±5 mm), ensuring the sample was flat and wrinkle-free, and vertically aligned. The tensile speed was 500mm / min. The tensile testing machine output the tensile strength value based on the sample width and thickness. Three tests were performed, and the average value was taken as the tensile strength (MPa) and elongation at break (%) in the MD / TD direction. Heat shrinkage:

[0097] Closed-cell temperature (air permeability method):

[0098] Cut a circular sample with a diameter of 50 mm and fix it in the sample slot of the hot stage of the gas transmission rate tester, ensuring that the edges are sealed. Start the heating program and record the real-time temperature and gas transmission rate data. When the transmission rate drops sharply to below 5% of the initial value, the corresponding temperature is the closed-cell temperature.

[0099] Film breaking temperature:

[0100] A 30mm long and 10mm wide diaphragm was tested using the TMA tensile method. The curve of the diaphragm length changing with temperature was recorded until the diaphragm broke. The temperature at which the diaphragm length increased instantaneously was the rupture temperature.

[0101] Thermal shrinkage rate:

[0102] The test was conducted according to the requirements of GB / T36363-2018. A 10cm × 10cm sample was cut, and the transverse (TD) and longitudinal (MD) widths were marked on the sample. The transverse and longitudinal widths were measured using a fully automatic image measuring projector (Kunshan Gaopin Precision Instrument Co., Ltd., GP-300C). The sample was held between two sealed A4 sheets of paper and placed in a 150℃ oven for 1 hour. After the sample returned to room temperature, the transverse and longitudinal widths were measured again using the fully automatic image measuring projector. Three measurements were taken, and the average value was recorded.

[0103] MD heat shrinkage rate (%) = (MD length before heating - MD length after heating) ÷ MD length before heating × 100;

[0104] TD heat shrinkage rate (%) = (TD length before heating - TD length after heating) ÷ TD length before heating × 100; Table 1

[0105] As shown in Table 1, modifying the microporous membrane surface with aromatic compounds containing alkenyl and ester groups can increase the membrane rupture temperature with minimal impact on the pore closure temperature, while also improving puncture resistance, tensile strength, and electrical conductivity to some extent. Experimental data from Examples 2 and 3, and Comparative Example 2, demonstrate that this invention can significantly improve membrane performance with relatively small amounts of modifying materials.

[0106] Experimental Example

[0107] The separators prepared in the examples and comparative examples were assembled into batteries, and the battery hit-pot defect rate and rate performance were tested.

[0108] Lithium cobalt oxide (LCO), conductive agent Super P, polyvinylidene fluoride (PVDF), and carbon nanotubes were mixed in a weight ratio of 96:2:2. N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under vacuum to obtain a positive electrode slurry with a solid content of 70 wt%. The obtained positive electrode slurry was uniformly coated onto a positive electrode current collector aluminum foil. The aluminum foil coated with the positive electrode slurry was dried at 90 °C, and then cold-pressed, cut, and slit to obtain the positive electrode sheet.

[0109] The negative electrode active material graphite, conductive additive Super P, sodium carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) were mixed in a weight ratio of 95:1.5:1.5:2. Deionized water was added, and the mixture was stirred in a vacuum mixer to obtain a negative electrode slurry with a solid content of 50 wt%. The negative electrode slurry was uniformly coated onto a negative electrode current collector copper foil. The copper foil was dried at 80 ℃, and then cold-pressed, cut, and slit. Finally, it was dried under vacuum at 110 ℃ for 12 h to obtain the negative electrode sheet.

[0110] Prepare the electrolyte in a dry argon atmosphere glove box: ethylene carbonate, methyl ethyl carbonate, and ethyl propionate are mixed in a ratio of 1:3:1, 3% fluoroethylene carbonate and 0.5% ethylene sulfate are mixed evenly to form the electrolyte, and then 1M LiPF6 is added and fully dissolved.

[0111] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. After welding the tabs, the battery is placed in an outer packaging foil-aluminum-plastic film, dried, and then tested for high potency. The prepared electrolyte is then injected, and the battery undergoes vacuum sealing, formation, capacity testing, degassing, shaping, and capacity testing to obtain a lithium-ion battery.

[0112] Hipot test: Apply 100V to the electrodes of the lithium-ion battery for 1 second. If the maximum leakage current is ≤1mA, the test is considered passed; otherwise, the Hipot is considered defective. 10,000 batteries are tested.

[0113] Cyclic performance test: The battery was charged at a constant current of 1C to 4.4V, then charged at a constant voltage of 0.05C. After resting for 10 minutes, it was discharged at 1C to 3V, and the capacity at this point was recorded as the initial capacity C0. The above charging process was repeated 300 times, and the discharge capacity C1 was recorded at this point. The capacity retention rate after 300 cycles was calculated as C1 / C0 * 100%. The test results are shown in Table 2.

[0114] Table 2

[0115] As can be seen from the data in Table 2, using the separator provided by this invention to prepare lithium batteries significantly reduces the Hipot defect rate and significantly improves the cycle stability of the battery.

[0116] The battery separator provided by this invention is not limited to the preparation method provided by this invention. Battery separators that conform to this invention and are obtained by other methods should be protected within the scope of the claims of this invention.

[0117] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the claims of the present invention.

Claims

1. A battery separator, comprising a microporous membrane and a coating, characterized in that, The microporous membrane is obtained by surface modification with an aromatic compound containing alkenyl and ester groups. The microporous membrane is surface-treated by surface irradiation or photodegradation to generate free radicals on its surface. The aromatic compound containing alkenyl and ester groups is dissolved in a solvent, and an initiator is added to prepare a modification solution. This modification solution is then contacted with the surface-treated microporous membrane, followed by ultraviolet irradiation. The aromatic compound containing alkenyl and ester groups constitutes 3%-13% of the mass of the microporous membrane. The aromatic compounds containing alkenyl and ester groups are one or more of the compounds shown in Formulas I-1 to I-6. Equation I-1; Equation I-2; Formula I-3; Equation I-4; Formula I-5; Formula I-6.

2. The method for preparing the battery separator according to claim 1, characterized in that, Includes the following steps: I. Preparation of modified microporous membranes: S1, dissolve the aromatic compound containing alkenyl and ester groups in claim 1 in a solvent, add an initiator, and prepare a modified solution; S2, the microporous membrane material is surface treated after being melt-cast, biaxially stretched, extracted and dried to generate free radicals on the surface of the microporous membrane. The modified solution is then brought into contact with the surface-treated microporous membrane, and then subjected to ultraviolet irradiation. After curing, it is cleaned, dried and subjected to secondary transverse stretching to obtain the modified microporous membrane. II. Coating Preparation: Step A: Prepare the coating slurry; Step B involves applying a coating slurry to at least one side of the modified microporous membrane.

3. The method for preparing the battery separator according to claim 2, characterized in that, In step S2, surface treatment is performed by surface irradiation or photodegradation. The surface irradiation is performed by a cobalt source or an electron accelerator, and the irradiation dose is 0.1 to 1 mgy. The ultraviolet irradiation conditions in step S2 are: ultraviolet wavelength of 200~450nm and time ≤60s.

4. The method for preparing the battery separator according to claim 2, characterized in that, In the modified solution of step S1, the content of aromatic compounds containing alkenyl and ester groups is 2-40 wt%, and the amount of initiator is 1-15 wt% of the weight of the aromatic compounds containing alkenyl and ester groups.

5. The method for preparing the battery separator according to claim 2, characterized in that, The initiator is at least one of benzoin ethers, α-hydroxy ketones, acetophenone derivatives, acylphosphine oxides, benzophenone, thioxanthones, and anthraquinones; The solvent is at least one of ethers, esters, and haloalkanes.

6. The method for preparing the battery separator according to claim 1, characterized in that, Includes the following steps: Step A': Prepare the coating slurry; Step B': Apply the coating slurry to at least one side of the finished microporous membrane and dry it; Step C': Dissolve the aromatic compound containing alkenyl and ester groups from claim 1 in a solvent, and then add an initiator to prepare a modified solution; Step D' involves surface-treating the membrane coated in step B' to generate free radicals on the surface of the microporous membrane. The modified solution is then brought into contact with the surface-treated microporous membrane, followed by ultraviolet irradiation. After curing, the membrane is cleaned and dried to obtain the modified diaphragm.

7. The method for preparing the battery separator according to claim 6, characterized in that, The coating thickness applied in step B' is 0.5μm~6μm.

8. A secondary battery, characterized in that, This includes the battery separator as described in claim 1 or the battery separator prepared by any one of claims 2 to 7.

Citation Information

Patent Citations

  • Novel cross-linked diaphragm, preparation method thereof, battery and electronic equipment

    CN114094284A

  • Modification method of porous polymer membrane, modified porous polymer membrane and application of modified porous polymer membrane

    CN119381693A