Preparation method and application of potassium modified carbon nitride bifunctional photocatalyst

By combining pre-impregnation and post-impregnation, the interlayer and electronic structures of potassium-modified carbon nitride were regulated, solving the problems of fast photogenerated electron-hole pair recombination rate and weak O2 activation ability of graphitic carbon nitride photocatalysts. This resulted in efficient organic matter degradation and hydrogen peroxide generation, improving the stability and performance of the catalyst.

CN121695908APending Publication Date: 2026-03-20Hefei Comprehensive Science Center Environmental Research Institute
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202511885896.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-15
Publication Date
2026-03-20

AI Technical Summary

Technical Problem

Existing graphitic carbon nitride photocatalysts have a fast photogenerated electron-hole pair recombination rate, small specific surface area, and weak O2 adsorption and activation ability, making it difficult to achieve the dual-function synergy of efficient organic matter degradation and hydrogen peroxide generation. Furthermore, the modification process is not well defined, leading to performance fluctuations.

Method used

By combining pre-impregnation and post-impregnation, the interlayer and electronic structures of potassium-modified carbon nitride were controlled, KN bonds were inserted to expand the interlayer spacing, and charge separation and O2 activation were optimized, thus preparing a bifunctional photocatalyst that can efficiently degrade organic matter and generate hydrogen peroxide.

Benefits of technology

It achieves efficient degradation of organic matter and generation of hydrogen peroxide, with stable catalyst performance, solving the problems of single function and ambiguous process in existing technologies, and improving photocatalytic performance and product generation rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121695908A_ABST
    Figure CN121695908A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a potassium modified graphite phase carbon nitride bifunctional photocatalyst, and belongs to the technical field of photocatalytic materials.According to the method, accurate regulation and control over a g-C3N4 interlayer structure, an electron energy band and surface active sites are achieved by regulating and controlling the KOH loading amount and the impregnation time sequence, on one hand, K < + > is inserted into the g-C3N4 interlayer through a K-N bond, and on the other hand, the KOH loading amount and the impregnation time sequence are adjusted and controlled; the interlayer spacing is enlarged, and photogenerated charge recombination is inhibited; on the other hand, the post-impregnation process can induce partial stripping of the g-C3N4 layered structure, so that the specific surface area is remarkably increased. The prepared catalyst has excellent rhodamine B (RhB) degradation and hydrogen peroxide generation performance under visible light, the degradation efficiency of 80 / KOH-coated C3N4 on RhB reaches 95.46%, the photocatalytic H2O2 generation rate reaches 18.7 mu mol / h, the performance retention rate exceeds 88% after five times of circulation, and the catalyst can be stably applied to the fields of environmental restoration and green chemical synthesis.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of photocatalytic material preparation and environmental governance, and particularly relates to a preparation method of a potassium-modified carbon nitride bifunctional photocatalyst and application thereof. BACKGROUND

[0002] The current global faces the double challenges of "water pollution treatment" and "green chemical synthesis": on the one hand, the organic dyes such as rhodamine B (RhB) discharged by the textile, printing and other industries are carcinogenic and difficult to be degraded by traditional processes, leading to the destruction of aquatic ecosystems; on the other hand, hydrogen peroxide (H2O2) as an oxidant without secondary pollution, its industrial anthraquinone production requires high temperature and high pressure, and the energy consumption accounts for more than 30%, and organic waste liquid is generated.

[0003] The photocatalytic technology can simultaneously realize "pollutant degradation" and "H2O2 generation" by using solar energy, and is regarded as a "one arrow with two targets" solution. Graphitic carbon nitride (g-C3N4) has become a core candidate material due to its advantages of no metal, suitable band gap (2.7 eV) and chemical stability, but its inherent defects restrict its application: the recombination rate of photo-generated electron-hole pairs is fast; the specific surface area is small, and the active sites are insufficient; the O2 adsorption and activation ability is weak, and it is difficult to efficiently generate H2O2.

[0004] In the existing modification strategies, potassium (K) doping can insert K-N bonds between the layers of g-C3N4, expand the interlayer spacing and regulate the electronic structure. However, there are two major bottlenecks in the existing research: ① single function, most of which focus on hydrogen production or single component degradation, and the "degradation-H2O2 production" bifunctional is not developed; ② unclear process, the difference between pre-impregnation (K and precursor co-calcination) and post-impregnation (K loaded on the synthesized g-C3N4) is not clear, resulting in uneven distribution of K and large performance fluctuations.

[0005] In order to overcome the above-mentioned bottlenecks, it is urgent to develop a K-modified g-C3N4 preparation method with controllable process and dual-function synergy, to realize the synergy of interlayer structure regulation, charge separation enhancement and O2 activation improvement by clarifying the impregnation sequence and parameters, and to break through the limitations of the existing technology. SUMMARY

[0006] The present application provides a preparation method of a potassium-modified carbon nitride bifunctional photocatalyst and application thereof, which can solve the problem of how to simultaneously optimize the interlayer structure, electronic band and surface activity of graphitic carbon nitride by a controllable potassium modification process in the prior art, to prepare a photocatalyst with efficient organic matter degradation and hydrogen peroxide generation bifunctional.

[0007] To solve the above problems, the present application provides a preparation method of a potassium-modified carbon nitride bifunctional photocatalyst, which comprises: Step one: take melamine into an alumina crucible with a cover, put it into a muffle furnace for heating, when the temperature is heated to 550 DEG C, keep it for a while, cool it to room temperature naturally, grind it with a agate mortar to get pure phase g-C3N4 powder; Step two: weigh KOH and dissolve it in anhydrous ethanol, mix KOH and anhydrous ethanol to form a homogeneous solution by magnetic stirring, add melamine, ultrasonic cavitation, then magnetic stirring until ethanol evaporates completely to form a solid, dry the obtained solid, and calcine to obtain x / K-C3N4, wherein x is the mass of KOH; Step three: mix the pure phase g-C3N4 prepared by melamine with KOH in an agate mortar, disperse the mixed powder in a mixture of 20 mL deionized water and anhydrous ethanol, ultrasonic for 1 h, magnetic stirring at 30 DEG C until the solvent evaporates completely, dry at 60 DEG C, then grind to obtain x / KOH@C3N4.

[0008] The application provides a preparation method of a potassium-modified carbon nitride bifunctional photocatalyst and application thereof, and has the following beneficial effects, but is not limited to the following: The difference between "pre-impregnation-calcination" and "post-impregnation-dispersion" is first determined: in step one, pre-impregnation is suitable for low K loading and can control the electronic structure; post-impregnation is suitable for high K loading and can realize layer peeling and specific surface area improvement, solving the performance fluctuation problem of the existing process.

[0009] In the method The K-N bond can be inserted into the interlayer of g-C3N4 to directly expand the interlayer spacing, which can reduce the interlayer charge transition resistance and inhibit the recombination rate of photo-generated electron-hole pairs, and the charge separation efficiency is a core determinant of photocatalytic performance, providing an electron transfer basis for subsequent degradation of pollutants and generation of H2O2.

[0010] Preferably, in steps two and three, the value of x includes 20, 40, 60, 80 or 100.

[0011] Preferably, in step one, the content of melamine is 10 g, the temperature is kept at 5 DEG C / min during the heating process, the holding temperature is 550 DEG C, and the holding time is 2 hours.

[0012] Preferably, in step two, the KOH content is 20 mg to 100 mg, and the anhydrous ethanol is 10 mL.

[0013] Preferably, in step two, the drying process is carried out at 60 DEG C for 12 hours.

[0014] Preferably, in step two, the ultrasonic treatment time after adding melamine is 1 hour, and the magnetic stirring time is 3 hours.

[0015] Preferably, in the step three, the volume ratio of deionized water to anhydrous ethanol in the mixed solvent is 1:1.

[0016] Preferably, the application further provides an application of the potassium-modified carbon nitride bifunctional photocatalyst, and in the application, the catalyst is used for catalytic degradation of organic dye rhodamine B under visible light irradiation.

[0017] Preferably, the application conditions are as follows: the catalyst is used in an amount of 10 mg, is dispersed in 50 mL of RhB aqueous solution with a concentration of 20 mg / L, and is reacted for 2 hours under xenon lamp irradiation.

[0018] Preferably, the catalyst is used for catalytic oxygen reduction to generate H2O2 under visible light irradiation, and the H2O2 generation rate of 80 / KOH@C3N4 is not less than 18 μmol / h. BRIEF DESCRIPTION OF DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the application, the drawings needed in the embodiment description will be briefly introduced. Obviously, the drawings in the following description are only some embodiments of the application, and other drawings can be obtained by those skilled in the art without creative labor.

[0020] Figure 1 X-ray diffraction patterns of pure-phase g-C3N4, x / K-C3N4 and x / KOH@C3N4; Figure 2 Scanning electron microscope images of some catalysts; Figure 3 H2O2 generation rate comparison chart of different catalysts; Figure 4 RhB degradation efficiency curve of different catalysts. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the application more clear, the technical solutions in the embodiments of the application will be described clearly and completely in the following with reference to the drawings which show the embodiments according to the application. It should be understood that the described embodiments are only some of the embodiments of the application, but not all the embodiments. Based on the embodiments described in the application, all other embodiments obtained by those skilled in the art without creative labor shall fall within the scope of protection of the application.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs; the terminology used in the description of the application herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application; the description and claims of the application herein are not to be limited to the specific embodiments described but are intended to cover all alternatives, modifications, and equivalents falling within the scope of the present application; the terms "comprising", "comprises" and "comprised of" as used herein are synonymous with "including", "includes" or "containing", "contains" and are inclusive or open-ended and do not exclude additional, unrecited elements or method steps; the terms "first", "second" and the like in the description do not denote any order, quantity, combination or importance, but rather are used to nomenclature various components and regions in the application, and "first" and "second" forms are not limited to the first and second forms, respectively. Thus, features having "first" "second" designations can include one or both of the features explicitly or implicitly. In the description of the application, "a plurality" means two or more, unless explicitly indicated to the contrary.

[0023] In the description of the present application, it needs to be understood that the terms "upper", "lower", "left", "right", "front", "back" and the like indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, and are only for the purpose of facilitating the description of the application and simplifying the description, and are not intended to indicate or imply that the devices or elements indicated must have a particular orientation, be constructed and operated in a particular orientation, and therefore cannot be understood as a limitation on the application.

[0024] In the description of the application, it should be noted that unless otherwise specified and limited, the terms "mounting", "connecting", "connection", "attaching" should be understood broadly, for example, it can be fixedly connected, or it can be detachably connected, or it can be integrally connected; it can be directly connected, or it can be indirectly connected through an intermediate medium; it can be the communication inside two elements. For those skilled in the art, the specific meaning of the above terms in the present application can be understood according to the specific circumstances.

[0025] It should be emphasized that when the term "comprising / including" is used in the present specification, it is used to explicitly indicate the presence of the features, integers, steps or components, but does not exclude the presence or addition of one or more other features, integers, steps, components or groups of features, integers, steps, components.

[0026] The application will be further described in detail below in conjunction with specific examples. The raw materials used are commercially available industrial grade or analytical pure reagents, and the experimental equipment not specifically mentioned is conventional laboratory equipment. The experimental environment is by default room temperature 25℃, normal pressure 1atm. The protection scope of the present application is not limited to the following examples.

[0027] Example 1: Preparation of pure phase g-C3N4

[0028] Select 10 g of melamine with purity ≥ 99%, select a 50 mL volume alumina crucible with a cover, ensure that the inner wall of the crucible is clean and free of impurities; evenly lay 10 g of melamine on the bottom of the alumina crucible, seal with a cover and put it into a muffle furnace, set the muffle furnace temperature program, heat to 550℃ at a constant heating rate of 5℃ / min, and keep the temperature constant for 2h to form g-C3N4; after the heat preservation is over, let the crucible cool down to room temperature with the furnace to avoid the structure of g-C3N4 being damaged due to sudden temperature change; take out the light yellow g-C3N4 solid product in the crucible, put it into an agate mortar and grind it thoroughly to get powder-like pure phase g-C3N4 for standby.

[0029] In the above, g-C3N4 is a typical polymer semiconductor, and the CN atoms in its structure form a highly delocalized π conjugated system through sp2 hybridization, which can effectively activate molecular oxygen to produce superoxide radicals for photocatalytic conversion of organic functional groups and photocatalytic degradation of organic pollutants.

[0030] Example 2: Preparation of x / K-C3N4 by pre-impregnation method

[0031] In this embodiment, x is the loading amount of the corresponding KOH, that is, how much KOH mass is added, and the value of x can be selected as 20, 40, 60, 80, 100, with the unit of mg.

[0032] This embodiment takes x=60mg (i.e. 60 / K-C3N4) as an example, and the preparation methods of the remaining x values only change the amount of KOH, and the remaining steps are completely consistent.

[0033] Take 60 mg of KOH with a purity of ≥98%, add the 60 mg of KOH to 10 mL of anhydrous ethanol with a purity of ≥99.7%, turn on the magnetic stirrer and stir slowly for 10 min until the KOH is completely dissolved in the anhydrous ethanol to form a uniform transparent KOH ethanol solution; add 10 g of the same batch of melamine used in Example 1 above to the KOH ethanol solution, place the melamine and KOH ethanol solution mixing system in an ultrasonic cleaner, and treat it with ultrasonic cavitation at a power of 80 W for 1 h to achieve uniform dispersion of the melamine and KOH solution. Control the temperature during ultrasonic treatment to be ≤30°C to prevent the ethanol from evaporating too quickly, causing the KOH to accumulate locally. Then transfer the mixing system to a constant temperature water bath, control the temperature to be 40°C, and continue magnetic stirring for 3 h until the anhydrous ethanol is completely evaporated, obtaining a white solid mixture; place the white solid mixture in an oven and dry it at a constant temperature of 60°C for 12 h to remove residual moisture; transfer the dried solid into an alumina crucible and perform calcination according to the calcination conditions of Example 1, i.e. 5°C / min to 550°C, and hold for 2 h; after the calcination product is naturally cooled, it is ground in a corundum mortar to obtain the target catalyst 60 / K-C3N4.

[0034] Similarly, take 20 mg, 40 mg, 80 mg, and 100 mg of KOH respectively, and repeat the above steps to prepare 20 / K-C3N4, 40 / K-C3N4, 60 / K-C3N4, and 80 / K-C3N4 catalysts in turn.

[0035] Example 3: Preparation of x / KOH@C3N4 by post-impregnation method

[0036] In this example, x is the loading amount of KOH, i.e. the amount of KOH added, and x can be selected as 20, 40, 60, 80, or 100, with units of mg.

[0037] This example takes x = 80 mg as an example, i.e. 80 / KOH@C3N4, and the preparation methods for the remaining x values only change the amount of KOH, and the remaining steps remain the same.

[0038] Take the pure phase g-C3N4 powder prepared in Example 1, which is prepared by 10 g of melamine in Example 1, and weigh 80 mg of KOH with a purity of ≥98%, put them together in a agate mortar, grind and mix for 10 min, ensure the uniformity of the mixture of the two solid powders, disperse the uniformly mixed solid powder in 20 mL of mixed solvent, which is prepared by deionized water and anhydrous ethanol in a volume ratio of 1:1; after mixing the prepared mixed solid powder and mixed solvent, the dispersion system formed is placed in an ultrasonic cleaner for 1 h, and also treated by ultrasonic cavitation at a power of 80 W for 1 h, after treatment, the dispersion system is placed in a 40℃ constant temperature water bath for magnetic stirring for at least 3 h, until the mixed solvent is completely evaporated to form a solid product, the solid product obtained in the above process is put into an oven, dried at 60℃ for 12 h, then taken out and ground in a agate mortar to obtain the target catalyst 80 / KOH@C3N4.

[0039] Similarly, weigh 20 mg, 40 mg, 60 mg, and 100 mg of KOH respectively, and repeat the above steps to prepare 20 / KOH@C3N4, 40 / KOH@C3N4, 60 / KOH@C3N4, and 100 / KOH@C3N4 catalysts in turn.

[0040] Example 4: Application of catalyst in RhB degradation

[0041] Take the materials prepared in Examples 1-3 as test catalysts, accurately weigh 10 mg of the corresponding catalyst, and disperse it in 50 mL of RhB aqueous solution with a concentration of 20 mg / L to obtain a uniform catalyst suspension; place the above suspension on a magnetic stirrer and stir for 30 min in a dark environment to ensure that the adsorption-desorption equilibrium between the catalyst and RhB molecules is reached; after the equilibrium of the suspension, irradiate it under a xenon lamp light source and continue to stir for 2 h, during which the reaction system is kept stable; after the reaction is completed, filter the suspension with a 0.45 μm filter membrane and detect the absorbance at a wavelength of 554 nm using a UV-visible spectrophotometer.

[0042] The detection results are shown in Table 1. Figure 4 As shown in Table 1, under the same external test conditions, the degradation efficiency of 80 / KOH@C3N4 on RhB is 95.46%.

[0043] In the examples of the present application, RhB is the abbreviation of Rhodamine B. The concentration is 20 mg / L, and this solution is often used as a reaction medium for testing the performance of catalysts. The chemical formula is C 28 H 31 ClN2O3, with a molecular weight of 479.02 g / mol, which is commonly used for fluorescent labeling, staining and as a photosensitizer in laboratories, etc.

[0044] Example 5: Application of catalyst in hydrogen peroxide production

[0045] The material prepared in Examples 1-3 was taken as the test catalyst, 50 mg of the catalyst was dispersed in 30 mL of a mixed solvent prepared by mixing methanol and deionized water at a volume ratio of 1:9; the mixed system was transferred into a 50 mL closed quartz reactor; the reactor was subjected to 3 cycles of freezing-vacuum pumping with a cold trap device equipped with liquid nitrogen to completely remove dissolved oxygen in the system; then pure O2 with a purity of ≥99.99% was introduced into the reactor, and the gas was continuously passed for 30 min to make the solution reach the O2 saturation state; the reactor was placed under a xenon lamp light source, and visible light with λ>420 nm was set, and the light intensity was controlled at 300 mW / cm 2 The reaction temperature was stabilized at 25°C by circulating cooling water, and the reaction was continued for 1 h; after the reaction was completed, the sample was centrifuged and separated, and the supernatant was taken and subjected to Ti 4 + H2O2 colorimetric method, detecting H2O2 concentration at 410 nm wavelength.

[0046] The detection results are shown in Table 1. Figure 4 As shown in Table 1, under the same external test conditions, the H2O2 production rate of 80 / KOH@C3N4 is 18.7 μmol / h.

[0047] Through the systematic verification of the above 5 examples, the following core conclusions can be drawn, which fully support the technical innovation and practicality of the present application: Process feasibility: the complete and feasible process of “pure phase g-C3N4 preparation (5 ℃ / min to 550 ℃ for 2 h) → pre-impregnation x / K-C3N4 (KOH 20-100 mg, 10 mL anhydrous ethanol, calcined under the same conditions) → post-impregnation x / KOH@C3N4 (1:1 mixed solvent, 30 ℃ stirring evaporation)” is clear, and the key parameters are clear and have high repeatability; Structure-performance correlation: it is confirmed that “impregnation timing and KOH loading” has a regulating effect on the structure of the product — pre-impregnation is suitable for low K loading (regulating electronic structure), post-impregnation is suitable for high K loading (inducing layer peeling and improving specific surface area), and the two achieve the dual optimization of “charge separation efficiency-active site number” in cooperation; Dual-functional optimal product: 80 / KOH@C3N4 is the optimal catalyst, which has a RhB degradation efficiency of 95.46% and a H2O2 production rate of 18.7 μmol / h, and has excellent cyclic stability, and can be stably applied to two fields of environmental remediation (dye wastewater treatment) and green chemical synthesis (H2O2 preparation), solving the bottleneck of “single function and unclear process” of the prior art.

[0048] The above embodiments only express several implementation manners of the present application, and the description is more specific and detailed, but it should not be understood as a limitation on the patent scope of the present application. It should be noted that for ordinary skilled persons in the art, without departing from the concept of the present application, several modifications and improvements can be made, which are within the protection scope of the present application.

Claims

1. A method for preparing a potassium-modified carbon nitride bifunctional photocatalyst, characterized in that, include: Step 1: Place melamine in a covered alumina crucible, heat it in a muffle furnace, and keep it at 550°C. After cooling naturally to room temperature, grind it with an agate mortar to obtain pure phase g-C3N4 powder. Step 2: Weigh KOH and dissolve it in anhydrous ethanol. Stir magnetically to form a homogeneous solution of KOH and anhydrous ethanol. Add melamine, sonicate, and then stir magnetically until the ethanol is completely evaporated to form a solid. Dry the obtained solid and calcine it to obtain x / K-C3N4, where x is the mass of KOH. Step 3: Grind and mix the pure phase g-C3N4 prepared with melamine and KOH in an agate mortar; disperse the mixed powder in 20 mL of a mixed solvent of deionized water and anhydrous ethanol, sonicate for 1 h, magnetically stir at 30 °C until the solvent is completely evaporated, dry at 60 °C, and then grind to obtain x / KOH@C3N4.

2. The method for preparing a potassium-modified carbon nitride bifunctional photocatalyst according to claim 1, characterized in that, In steps two and three, the value of x can be 20, 40, 60, 80 or 100.

3. The method for preparing a potassium-modified carbon nitride bifunctional photocatalyst according to claim 1, characterized in that, In step one, the melamine content is 10g. During the heating process, the temperature is maintained at 5℃ / min for heating, the holding temperature is 550℃, and the holding time is 2 hours.

4. The method for preparing a potassium-modified carbon nitride bifunctional photocatalyst according to claim 1, characterized in that, In step two, the amount of KOH weighed is 20mg to 100mg, and the amount of anhydrous ethanol is 10mL.

5. The method for preparing a potassium-modified carbon nitride bifunctional photocatalyst according to claim 1, characterized in that, In step two, the drying process is carried out at 60°C for 12 hours.

6. The method for preparing a potassium-modified carbon nitride bifunctional photocatalyst according to claim 1, characterized in that, In step two, the ultrasonic treatment time after adding melamine is 1 hour, and the magnetic stirring time is 3 hours.

7. The method for preparing a potassium-modified carbon nitride bifunctional photocatalyst according to claim 1, characterized in that, In step three, the volume ratio of deionized water to anhydrous ethanol in the mixed solvent is 1:

1.

8. The application of a potassium-modified carbon nitride bifunctional photocatalyst, prepared according to any one of claims 1 to 7, characterized in that, The catalyst is used to catalytically degrade the organic dye Rhodamine B under visible light irradiation.

9. The application of the potassium-modified carbon nitride bifunctional photocatalyst according to claim 8, characterized in that, The application conditions were as follows: 10 mg of catalyst was dispersed in 50 mL of 20 mg / L RhB aqueous solution and reacted under xenon lamp irradiation for 2 hours.

10. The application of the potassium-modified carbon nitride bifunctional photocatalyst according to claim 8, characterized in that, The catalyst is used to catalyze the reduction of oxygen to H2O2 under visible light irradiation, wherein the H2O2 generation rate of 80 / KOH@C3N4 is not less than 18 μmol / h.

Citation Information

Patent Citations

  • Novel photocatalyst K-g-C3N4 as well as preparation and application thereof

    CN107774294A

  • High-crystallinity carbon nitride, preparation method thereof and application of high-crystallinity carbon nitride in photocatalytic production of hydrogen peroxide

    CN116654881A

  • K / O co-doped and cyano-grafted graphite phase carbon nitride material as well as preparation method and application thereof

    CN119565655A

  • Photocatalytic method and system for the production of hydrogen peroxide

    WO2022243496A1