Lithium iron phosphate battery fast charging performance determination method and fast charging battery design method
By constructing an association model to quickly locate and design the fast-charging performance of lithium iron phosphate batteries, the problem of low efficiency in locating and designing the fast-charging performance of lithium-ion batteries in existing technologies is solved, and fast and economical fast-charging battery design is realized.
Patent Information
- Application Number
- CN202511663542.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-13
- Publication Date
- 2026-03-24
AI Technical Summary
The fast-charging performance of lithium-ion batteries is affected by various parameters such as negative electrode material, electrode surface density, and electrolyte conductivity. Existing methods are costly and inefficient, making it difficult to quickly identify and design lithium-ion batteries suitable for fast charging.
A correlation model was constructed between the cumulative percentage of the negative electrode active material, the negative electrode coating density, the negative electrode compaction density, and the electrolyte conductivity using Raman surface scanning. By adjusting these parameters, the fast-charging performance of lithium iron phosphate batteries was quickly located and designed. The charging rate that the lithium-ion battery can support was calculated using the formula C=[2.16×(R10+R90)-0.3×G-8×P+21.5]×σ/10.
It enables rapid positioning of the fast-charging performance of lithium-ion batteries, shortens the design cycle, allows adjustment of battery parameters according to different needs, meets different fast-charging requirements, and reduces R&D costs.
Smart Images

Figure CN121723646A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium iron phosphate battery technology, and in particular to a method for determining the fast-charging performance of lithium iron phosphate batteries and a fast-charging battery design method. Background Technology
[0002] Compared to the rapid refueling of traditional internal combustion engine vehicles, the rapid charging of lithium-ion batteries (LIBs) is one of the key factors limiting the widespread adoption of electric vehicles. Therefore, charging speed is a crucial technology that must be overcome for electric vehicles to replace traditional gasoline-powered vehicles, and it is also a very important indicator affecting user experience.
[0003] Electrode materials are crucial for fast charging, as their performance at high rates significantly impacts the battery's fast-charging capability. The poor kinetic performance of the lithium-ion battery's negative electrode leads to high internal resistance, thus affecting its fast-charging and cycle performance. Graphite negative electrodes, with their insufficient ion channels and low potential, result in slow ion migration at high rates, making them prone to overpotential. This can lead to lithium dendrite growth on the negative electrode surface, causing capacity loss and posing safety hazards.
[0004] In a specific power battery system, the key factors determining its charging speed are the negative electrode and the electrolyte. The fast-charging performance of lithium-ion batteries is affected by many technical parameters, including the defect degree of the negative electrode active material, the electrode surface density, the compaction density, and the electrolyte conductivity, which are interrelated and mutually restrictive. Fabricating a set of lithium-ion batteries for each variable and conducting charge-discharge experiments is costly, inefficient in variable selection, and results in a long battery design and development cycle. Summary of the Invention
[0005] The purpose of this invention is to overcome the deficiencies in the existing technologies and provide a method for determining the fast-charging performance of lithium iron phosphate batteries and a fast-charging battery design method, aiming to quickly determine the fast-charging performance of lithium-ion batteries; quickly design lithium-ion batteries suitable for different fast-charging needs; and shorten the design cycle of fast-charging batteries.
[0006] The technical solution adopted to achieve the purpose of this invention is: One objective of this invention is to provide a method for determining the fast-charging performance of a lithium iron phosphate battery, comprising the following steps: Raman surface scanning was established to achieve a cumulative percentage of Raman spectroscopy for the negative electrode active material reaching two preset values. D / I G A correlation model between the values, areal density of the negative electrode coating, compaction density of the negative electrode, conductivity of the electrolyte, and the charging rate that a lithium-ion battery can support. Raman surface scanning of lithium iron phosphate batteries yielded Raman I values where the cumulative percentage of the anode active material reached two preset values.D / I G Value, areal density of negative electrode coating, compaction density of negative electrode, and conductivity of electrolyte; The fast-charging performance of lithium iron phosphate batteries is determined by calculating the charging rate that lithium-ion batteries can support based on the correlation model.
[0007] Among them, the cumulative percentage of the Raman surface scanned negative electrode active material reaches two preset values of Raman I. D / I G The values are R10, representing 10% of the cumulative quantity, and R90, representing 90% of the cumulative quantity.
[0008] Wherein, the correlation model C = [2.16 × (R10 + R90) - 0.3 × G - 8 × P + 21.5] × σ / 10; Where C represents the charging rate that the lithium-ion battery can support, and R10 and R90 are the Raman I values corresponding to 10% and 90% of the cumulative percentage of Raman-scanned negative electrode active material, respectively. D / I G Value; G is the negative electrode coating surface density, unit mg / cm³. 2 P represents the compacted density of the negative electrode sheet after rolling, in g / cm³. 3 σ represents the electrolyte conductivity, measured in mS / cm.
[0009] Specifically, when C≥10, the lithium-ion battery has a rate performance of 10C or higher; when 6≤C≤10, the lithium-ion battery has a rate performance of 6C-10C; when 4≤C≤6, the lithium-ion battery has a rate performance of 4C-6C; and when C≤4, the lithium-ion battery has a rate performance of less than 4C.
[0010] Another objective of this invention is to provide a design method for a lithium iron phosphate fast-charging battery, comprising the following steps: Raman surface scanning was established to achieve a cumulative percentage of Raman spectroscopy for the negative electrode active material reaching two preset values. D / I G A correlation model between the values, areal density of the negative electrode coating, compaction density of the negative electrode, conductivity of the electrolyte, and the charging rate that a lithium-ion battery can support. Based on the aforementioned correlation model, to achieve the expected charging rate that the lithium-ion battery can support, the Raman surface scan percentage of the cumulative quantity of the negative electrode active material must reach two preset values. D / I G Value, areal density of negative electrode coating, compaction density of negative electrode, and conductivity of electrolyte.
[0011] Among them, the cumulative percentage of the Raman surface scanned negative electrode active material reaches two preset values of Raman I. D / IG The values are R10, representing 10% of the cumulative quantity, and R90, representing 90% of the cumulative quantity.
[0012] Wherein, the correlation model C = [2.16 × (R10 + R90) - 0.3 × G - 8 × P + 21.5] × σ / 10; Where C represents the charging rate that the lithium-ion battery can support, and R10 and R90 are the Raman I values corresponding to 10% and 90% of the cumulative percentage of Raman-scanned negative electrode active material, respectively. D / I G Value; G is the negative electrode coating surface density, unit mg / cm³. 2 P represents the compacted density of the negative electrode sheet after rolling, in g / cm³. 3 σ represents the electrolyte conductivity, measured in mS / cm.
[0013] Specifically, the lithium-ion battery's charge rate C value in the correlation model is adjusted by adjusting one or more of the following: the cumulative percentage of Raman-scanned negative electrode active material reaches 10% and 90% (R10 and R90); the negative electrode coating density (G); the compaction density of the negative electrode sheet after rolling (P); and the electrolyte conductivity (σ). This allows the lithium-ion battery to have the required rate performance.
[0014] Specifically, when C≥10, the lithium-ion battery has a rate performance of 10C or higher; when 6≤C≤10, the lithium-ion battery has a rate performance of 6C-10C; when 4≤C≤6, the lithium-ion battery has a rate performance of 4C-6C; and when C≤4, the lithium-ion battery has a rate performance of less than 4C.
[0015] The negative electrode active material is one or more of artificial graphite and natural graphite.
[0016] This invention constructs a mathematical model, C=[2.16×(R10+R90)-0.3×G-8×P+21.5]×σ / 10, to correlate parameters closely related to the fast-charging performance of lithium-ion batteries: the Raman spectral density corresponding to 10% of the cumulative Raman distribution of graphite powder. D / I G R10, Raman I value corresponding to 90% cumulative distribution of the surface scan Raman spectroscopy of graphite powder D / I GThe values R90, electrode coating areal density, electrode coating compaction density, and electrolyte conductivity enable rapid identification of the fast-charging performance of lithium-ion batteries, reducing lengthy subsequent R&D work. This allows for the rapid determination of the applicable charging rate for the lithium-ion battery under a given design, guiding the determination of the battery's fast-charging mode. When C ≥ 10, the lithium-ion battery has a rate performance of 10C or higher; when 6 ≤ C ≤ 10, the lithium-ion battery has a rate performance of 6C-10C; when 4 ≤ C ≤ 6, the lithium-ion battery has a rate performance of 4C-6C; and when C ≤ 4, the lithium-ion battery has a rate performance of less than 4C.
[0017] Simultaneously, based on the constructed mathematical model C=[2.16×(R10+R90)-0.3×G-8×P+21.5]×σ / 10, a design method for lithium iron phosphate fast-charging batteries is provided. This method enables the design of different negative electrode parameters and electrolyte parameters for different fast-charging requirements, thereby achieving the corresponding fast-charging objectives. By simultaneously adjusting the Raman value of the negative electrode active material, the areal density of the negative electrode sheet, the compaction density of the negative electrode sheet, and the conductivity of the electrolyte, the dynamic performance of the lithium-ion battery negative electrode can be adjusted, thereby reducing the battery's internal resistance and fast-charging performance. This allows for the design or provision of different lithium-ion batteries according to different fast-charging requirements. Attached Figure Description
[0018] Figure 1 This is a flowchart of the method for determining the fast charging performance of lithium iron phosphate batteries according to the present invention.
[0019] Figure 2 This is a flowchart of the lithium iron phosphate fast-charging battery design method of the present invention. Detailed Implementation
[0020] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0021] See Figure 1 As shown, this embodiment of the invention provides a method for determining the fast-charging performance of a lithium iron phosphate battery, including: Raman surface scanning was established to achieve a cumulative percentage of Raman spectroscopy for the negative electrode active material reaching two preset values. D / I G A correlation model between the values, areal density of the negative electrode coating, compaction density of the negative electrode, conductivity of the electrolyte, and the charging rate that a lithium-ion battery can support. Raman surface scanning of lithium iron phosphate batteries yielded Raman I values where the cumulative percentage of the anode active material reached two preset values. D / I G Value, areal density of negative electrode coating, compaction density of negative electrode, and conductivity of electrolyte; The fast-charging performance of lithium iron phosphate batteries is determined by calculating the charging rate that lithium-ion batteries can support based on the correlation model.
[0022] Wherein, the correlation model is C = [2.16 × (R10 + R90) - 0.3 × G - 8 × P + 21.5] × σ / 10. In the model, R10 and R90 represent the Raman spectral density (R10) of the negative electrode active material, respectively. D / I G The values are calculated as follows: R10 represents the cumulative distribution value at 10%; R90 represents the cumulative distribution value at 90%. Specifically, R10 represents the Raman value corresponding to a cumulative percentage of 10% of the negative electrode active material using Raman surface scanning, and R9 represents the Raman value corresponding to the same cumulative percentage. G represents the negative electrode coating surface density, calculated as the weight of the negative electrode powder divided by the coating area, in mg / cm². 2 P represents the compacted density of the negative electrode sheet after roller pressing, calculated as the negative electrode coating surface density G / negative electrode powder thickness, in g / cm³. 3 σ represents the electrolyte conductivity, measured in mS / cm. C represents the charge rate that the lithium-ion battery can support, calculated as C = 60 / T, where T is the charging time, measured in minutes.
[0023] Among them, Raman surface scanning of the anode active material Raman I D / I G The value can be measured using a Raman spectrometer.
[0024] Specifically: when C≥10, the lithium-ion battery has a rate performance of 10C or higher; when 6≤C≤10, the lithium-ion battery has a rate performance of 6C-10C; when 4≤C≤6, the lithium-ion battery has a rate performance of 4C-6C; and when C≤4, the lithium-ion battery has a rate performance of less than 4C.
[0025] See Figure 2 As shown, embodiments of the present invention also provide a design method for a lithium iron phosphate fast-charging battery, including: Raman surface scanning was established to achieve a cumulative percentage of Raman spectroscopy for the negative electrode active material reaching two preset values. D / I G A correlation model between the values, areal density of the negative electrode coating, compaction density of the negative electrode, conductivity of the electrolyte, and the charging rate that a lithium-ion battery can support. Based on the aforementioned correlation model, to achieve the expected charging rate that the lithium-ion battery can support, the Raman surface scan percentage of the cumulative quantity of the negative electrode active material must reach two preset values. D / I GValue, areal density of negative electrode coating, compaction density of negative electrode, and conductivity of electrolyte.
[0026] Wherein, the correlation model is C = [2.16 × (R10 + R90) - 0.3 × G - 8 × P + 21.5] × σ / 10; In the model, R10 and R90 represent the Raman spectral density (R10) of the negative electrode active material, respectively. D / I G The values are calculated as follows: R10 represents the cumulative distribution value at 10%; R90 represents the cumulative distribution value at 90%. Specifically, R10 represents the Raman value corresponding to a cumulative percentage of 10% of the negative electrode active material using Raman surface scanning, and R9 represents the Raman value corresponding to the same cumulative percentage. G represents the negative electrode coating surface density, calculated as the weight of the negative electrode powder divided by the coating area, in mg / cm². 2 P represents the compacted density of the negative electrode sheet after roller pressing, calculated as the negative electrode coating surface density G / negative electrode powder thickness, in g / cm³. 3 σ represents the electrolyte conductivity, measured in mS / cm. C represents the charge rate that the lithium-ion battery can support, calculated as C = 60 / T, where T is the charging time, measured in minutes.
[0027] Among them, Raman surface scanning of the anode active material Raman I D / I G The value can be measured using a Raman spectrometer.
[0028] Specifically, the following steps are used to determine the battery design process: Raman spectroscopy for determining the surface-scanned active material of graphite anode powder D / I G Values, the distribution of statistical values accounting for 10% of the values, R10; determining the Raman spectroscopy of the graphite anode powder surface-scanned anode active material. D / I G The value, the statistical distribution of the 90% percentile value R90; determine the areal density G of the negative electrode, in mg / cm³. 2 Determine the compaction density P of the negative electrode sheet, in g / cm³. 3 Determine the conductivity σ of the electrolyte, in mS / cm; According to the formula C=[2.16×(R10+R90)-0.3×G-8×P+21.5]×σ / 10, the supporting charging rate of the corresponding lithium iron phosphate battery can be determined, and the fast charging battery design can be carried out.
[0029] Specifically, by adjusting the performance parameters of the negative electrode active material, the process parameters of the negative electrode sheet, or the performance parameters of the electrolyte, the rate performance (C) of the lithium-ion battery can meet the design requirements. In other words, by adjusting one or more of R10, R90, G, P, and σ, the C value in the formula can be adjusted, thereby enabling the lithium-ion battery to have the required rate performance (fast charging performance).
[0030] Specifically: when C≥10, the lithium-ion battery has a rate performance of 10C or higher; when 6≤C≤10, the lithium-ion battery has a rate performance of 6C-10C; when 4≤C≤6, the lithium-ion battery has a rate performance of 4C-6C; and when C≤4, the lithium-ion battery has a rate performance of less than 4C.
[0031] In some optional embodiments, the negative electrode active material is one or more of artificial graphite and natural graphite; in some optional embodiments, the particle size of the negative electrode active material is 3 μm ≤ D10 ≤ 8 μm, preferably 4 μm ≤ D10 ≤ 7 μm. In some optional embodiments, the particle size of the negative electrode active material is 8 μm ≤ D50 ≤ 17 μm, preferably 9 μm ≤ D50 ≤ 14 μm. In some optional embodiments, the particle size of the negative electrode active material is 18 μm ≤ D90 ≤ 40 μm, preferably 20 μm ≤ D90 ≤ 35 μm. In some optional embodiments, the specific surface area of the negative electrode active material is 0.5 m². 2 / g-3 m 2 / g, preferably 0.8 m 2 / g-2 m 2 / g. In some alternative embodiments, the OI value of the negative electrode active material is 1-9, preferably 2-6.
[0032] In some optional embodiments, the positive electrode active material is lithium iron phosphate, with a particle size of 0.3 μm ≤ D50 ≤ 2 μm. Optionally, the lithium iron phosphate material has a particle size of 0.5 μm ≤ D50 ≤ 1.5 μm.
[0033] In some optional embodiments, the electrolyte contains a first lithium salt, which is selected from any one of lithium hexafluorophosphate, lithium bisfluorosulfonylimide, lithium bistrifluoromethanesulfonylimide, lithium difluorophosphate, and lithium difluorooxalateborate. The mass content of the lithium salt in the electrolyte is between 8wt% and 14wt%. When the mass content of the first lithium salt is within the above range, it helps to improve the conductivity of the electrolyte and improve the fast charging performance of the battery cell.
[0034] In some optional embodiments, the electrolyte contains a second lithium salt, which is selected from any one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, and lithium difluorooxalateborate. The mass content of the lithium salt in the electrolyte is between 1 wt% and 5 wt%. When the mass content of the second lithium salt is within the above range, it helps to further improve the conductivity of the electrolyte and improve the fast charging performance of the battery cell.
[0035] In some alternative embodiments, the electrolyte solvent is selected from two or more combinations of ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, ethyl acrylate, ethyl formate, ethyl acetate, ethyl propionate, and methyl propionate.
[0036] The additive is selected from any one or a combination of two or more of vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, vinyl sulfite, methane disulfonate, tris(trimethylsilane) phosphate, and polystyrene. The content of the electrolyte additive shall not exceed 8%.
[0037] In some optional embodiments, the Raman I value corresponding to a cumulative percentage of 10% of the negative electrode active material is determined by Raman surface scanning. D / I G The value R10 corresponds to a range of 0-0.2; the Raman I value is the value corresponding to the cumulative percentage of the negative electrode active material reaching 90% using Raman surface scanning. D / I G The corresponding range for R9 is 0.1-0.7. Example
[0038] Positive electrode preparation: Lithium iron phosphate (LFP), conductive carbon black Super-P, carbon nanotubes (CNT), and polyvinylidene fluoride (PVDF) binder are mixed in NMP at a weight ratio of 90%:2%:3%:5% to form a lithium iron phosphate cathode slurry. After thorough stirring and viscosity adjustment, a uniformly mixed cathode slurry with a solid content of 65% is obtained. The lithium iron phosphate cathode slurry is coated on both sides of a current collector aluminum foil according to a set double-sided surface density to form an electrode sheet at a coating speed of 5 m / min. The electrode sheets are then placed in an oven for drying. The dried cathode sheets are then rolled according to the designed compaction density to obtain a lithium iron phosphate cathode electrode sheet.
[0039] Negative electrode preparation: A graphite slurry is formed by mixing graphite, conductive carbon black, CMC binder, and SBR binder in water at a weight ratio of 94%:2%:1.5%:2.5%. After thorough stirring and viscosity adjustment, a uniformly mixed negative electrode slurry with a solid content of 55% is obtained. The graphite slurry is then coated onto both sides of a current collector copper foil at a double-sided density to form an electrode sheet at a coating speed of 8 m / min. The electrode sheets are then sequentially placed in an oven for drying. After drying, the negative electrode sheets are rolled according to the designed compaction density to obtain a graphite negative electrode sheet.
[0040] Electrolyte: The electrolyte contains lithium salt, additives and organic solvents. The electrolyte solvent is mixed in a 50%:50% ratio of vinyl acetate (EC) and diethyl carbonate (DEC). The amount of lithium salt lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI) added is 13%, and the content of additives in the electrolyte is no more than 8%.
[0041] Diaphragm: A 7+3+2μm polyethylene film with single-sided ceramic coating and single-sided adhesive was used as the diaphragm.
[0042] Preparation of lithium-ion batteries: The positive electrode, separator, and negative electrode are wound in sequence, with the separator positioned between the positive and negative electrodes. The positive and negative electrodes, together with the polyethylene separator, form an electrode assembly, thus creating a dry cell. Electrolyte is injected into the dry cell to complete the formation process and obtain a lithium-ion battery.
[0043] Maximum charging rate test: The lithium-ion battery was fully charged at 25°C with different charging rates, then discharged with a small current, and then fully charged again with the corresponding charging rate. The battery was then disassembled to observe whether lithium plating was present at the negative electrode interface. If lithium plating was present, it indicated that the negative electrode did not meet the charging rate requirement. The charging rate was then gradually reduced to observe the negative electrode interface until no lithium plating was present on the surface of the negative electrode. This was the maximum charging rate corresponding to the battery.
[0044] Raman value testing method: Place the sample to be tested on the sample holder, ensuring it is as flat and smooth as possible to guarantee the accuracy of the spectral data. Determine the instrument parameters, selecting appropriate laser wavelength, power, and detector parameters based on the sample characteristics to ensure clear and stable spectral signals. Perform a background scan to eliminate interference from the instrument's background signal on the sample signal. Place the sample on the sample holder for testing, performing single-point measurements. Process and analyze the 400 spectral data points obtained using spectral instrument software or specialized processing software to obtain 400 Raman value data points. Determine the Raman value of the graphite anode powder surface-scanned anode active material. The statistical distribution of the 10% percentile is R10, and the statistical distribution of the 90% percentile is R90. Raman value = I D / IG I D 1350cm -1 The intensity of peak D, I G 1580cm -1 The intensity of peak G.
[0045] Detailed test method for areal density: The area and corresponding weight of the electrode are accurately measured using an analytical balance and a ruler. The areal density of the electrode is calculated by dividing the measured weight by the area. Electrode cutting must ensure measurement accuracy. The unit of areal density is mg / cm³. 2 .
[0046] Detailed test method for compacted density: The thickness of the electrode sheet and the current collector after rolling is measured using a thickness gauge (such as a micrometer or ten-thousand-point caliper). The compaction density of the electrode sheet can be obtained by dividing the areal density by the difference between these two thicknesses. The unit of compaction density is g / cm³. 3 Conductivity testing methods: After calibrating the instrument with a standard KCl solution (0.1 mol / L, conductivity 12.88 mS / cm at 25°C), immerse the electrode in the electrolyte to be tested and read the stabilized conductivity value.
[0047] In Example 1, the graphite powder had an R10 value of 0.15 and an R90 value of 0.5, and an areal density of 14 mg / cm³. 2 The compacted density is 1.4 g / cm³. 3 The electrolyte conductivity is 16 mS / cm. Example 2
[0048] The difference from Example 1 is that the electrolyte conductivity is 14 mS / cm. Example 3
[0049] The difference from Example 1 is that the graphite powder has an R10 value of 0.1 and an R90 value of 0.3, and the electrolyte conductivity is 14 mS / cm. Example 4
[0050] The difference from Example 1 is that the compaction density is 1.5 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 5
[0051] The difference from Example 1 is that the areal density is 18 mg / cm³. 2 The electrolyte conductivity is 14 mS / cm. Example 6
[0052] The difference from Example 1 is that the areal density is 16 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 7
[0053] The difference from Example 1 is that the areal density is 18 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 The electrolyte conductivity is 15 mS / cm. Example 8
[0054] The difference from Example 1 is that the areal density is 18 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 9
[0055] The difference from Example 1 is that the areal density is 18 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 The electrolyte conductivity is 13 mS / cm. Example 10
[0056] The difference from Example 1 is that the graphite powder has an R10 value of 0.1 and an R90 value of 0.3, and an areal density of 18 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 11
[0057] The difference from Example 1 is that the areal density is 18 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 The electrolyte conductivity is 12 mS / cm. Example 12
[0058] The difference from Example 1 is that the areal density is 18 mg / cm³. 2 The compacted density is 1.6 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 13
[0059] The difference from Example 1 is that the areal density is 18 mg / cm³. 2 The compacted density is 1.65 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 14
[0060] The difference from Example 1 is that the density is 20 mg / cm³. 2 The compacted density is 1.6 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 15
[0061] The difference from Example 1 is that the graphite powder has an R10 value of 0.1 and an R90 value of 0.3, and a density of 20 mg / cm³. 2 The compacted density is 1.65 g / cm³. 3 The electrolyte conductivity is 14 mS / cm. Example 16
[0062] The difference from Example 1 is that the graphite powder has an R10 value of 0.1 and an R90 value of 0.3, and a density of 20 mg / cm³. 2 The compacted density is 1.7 g / cm³. 3 The electrolyte conductivity is 14 mS / cm.
[0063] The cell parameters and battery performance test results of the embodiment are shown in Table 1.
[0064] Table 1 Raman value R10 Raman value R90 <![CDATA[Areal density (mg / cm 2 )]]> <![CDATA[Compaction density (g / cm 3 )]]> Electrolyte conductivity (mS / cm) Calculated value of C Ratio performance Example 1 0.15 0.5 14 1.4 16 12.0 12.0C Example 2 0.15 0.5 14 1.4 14 10.5 10.5C Example 3 0.1 0.3 14 1.4 14 9.8 9.8C Example 4 0.15 0.5 14 1.5 14 9.4 9.5C Example 5 0.15 0.5 18 1.4 14 8.8 8.8C Example 6 0.15 0.5 16 1.5 14 8.6 8.5C Example 7 0.15 0.5 18 1.5 15 8.3 8.0C Example 8 0.15 0.5 18 1.5 14 7.7 7.5C Example 9 0.15 0.5 18 1.5 13 7.2 7.0C Example 10 0.1 0.3 18 1.5 14 7.0 7.0C Example 11 0.15 0.5 18 1.5 12 6.6 6.6C Example 12 0.15 0.5 18 1.6 14 6.6 6.5C Example 13 0.15 0.5 18 1.65 14 6.0 6.0C Example 14 0.15 0.5 20 1.6 14 5.8 5.8C Example 15 0.1 0.3 20 1.65 14 4.4 4.5C Example 16 0.1 0.3 20 1.7 14 3.9 3.9C The table above shows that a high defect degree in the negative electrode facilitates rapid lithium-ion transport and reduces transport resistance. Higher areal density in the negative electrode increases the lithium-ion insertion / extraction pathway, intensifies concentration polarization, and increases resistance to lithium-ion insertion and extraction, thus affecting fast-charging performance. As compaction density increases, the material's wettability to the electrolyte weakens, increasing contact resistance and hindering rapid lithium-ion transport.
[0065] In summary, it can be seen that the charging rate of a lithium-ion battery can be quickly determined by the formula C=[2.16×(R10+R90)-0.3×G-8×P+21.5]×σ / 10. By adjusting one or more of R10, R90, G, P and σ, the value of C in the formula can be adjusted, thereby enabling the lithium-ion battery to have the required rate performance (fast charging performance).
[0066] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. It will be apparent to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of the equivalents of the claims be included within the invention.
[0067] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for determining the fast-charging performance of lithium iron phosphate batteries, characterized in that, Including steps: Raman surface scanning was established to achieve a cumulative percentage of Raman spectroscopy for the negative electrode active material reaching two preset values. D / I G A correlation model between the values, areal density of the negative electrode coating, compaction density of the negative electrode, conductivity of the electrolyte, and the charging rate that a lithium-ion battery can support. Raman surface scanning of lithium iron phosphate batteries yielded Raman I values where the cumulative percentage of the anode active material reached two preset values. D / I G Value, areal density of negative electrode coating, compaction density of negative electrode, and conductivity of electrolyte; The fast-charging performance of lithium iron phosphate batteries is determined by calculating the charging rate that lithium-ion batteries can support based on the correlation model.
2. The method for determining the fast-charging performance of a lithium iron phosphate battery according to claim 1, characterized in that, The cumulative percentage of the Raman surface scanned negative electrode active material reaches two preset values. D / I G The values are R10, representing 10% of the cumulative quantity, and R90, representing 90% of the cumulative quantity.
3. The method for determining the fast-charging performance of a lithium iron phosphate battery according to claim 2, characterized in that, The correlation model is C = [2.16 × (R10 + R90) - 0.3 × G - 8 × P + 21.5] × σ / 10; Where C represents the charging rate that the lithium-ion battery can support, and R10 and R90 are the Raman I values corresponding to 10% and 90% of the cumulative percentage of Raman-scanned negative electrode active material, respectively. D / I G Value; G is the negative electrode coating surface density, unit mg / cm³. 2 P represents the compacted density of the negative electrode sheet after rolling, in g / cm³. 3 σ represents the electrolyte conductivity, measured in mS / cm.
4. The method for determining the fast-charging performance of a lithium iron phosphate battery according to claim 3, characterized in that, When C≥10, lithium-ion batteries have a rate performance of 10C or higher; when 6≤C≤10, lithium-ion batteries have a rate performance of 6C-10C; when 4≤C≤6, lithium-ion batteries have a rate performance of 4C-6C; when C≤4, lithium-ion batteries have a rate performance of less than 4C.
5. A design method for a lithium iron phosphate fast-charging battery, characterized in that, Including the following steps: Raman surface scanning was established to achieve a cumulative percentage of Raman spectroscopy for the negative electrode active material reaching two preset values. D / I G A correlation model between the values, areal density of the negative electrode coating, compaction density of the negative electrode, conductivity of the electrolyte, and the charging rate that a lithium-ion battery can support. Based on the aforementioned correlation model, to achieve the expected charging rate that the lithium-ion battery can support, the Raman surface scan percentage of the cumulative quantity of the negative electrode active material must reach two preset values. D / I G Value, areal density of negative electrode coating, compaction density of negative electrode, and conductivity of electrolyte.
6. The lithium iron phosphate fast-charging battery design method according to claim 5, characterized in that, The cumulative percentage of the Raman surface scanned negative electrode active material reaches two preset values. D / I G The values are R10, representing 10% of the cumulative quantity, and R90, representing 90% of the cumulative quantity.
7. The design method for a lithium iron phosphate fast-charging battery according to claim 6, characterized in that, The correlation model is C = [2.16 × (R10 + R90) - 0.3 × G - 8 × P + 21.5] × σ / 10; Where C represents the charging rate that the lithium-ion battery can support, and R10 and R90 are the Raman I values corresponding to 10% and 90% of the cumulative percentage of Raman-scanned negative electrode active material, respectively. D / I G Value; G is the negative electrode coating surface density, unit mg / cm³. 2 P represents the compacted density of the negative electrode sheet after rolling, in g / cm³. 3 σ represents the electrolyte conductivity, measured in mS / cm.
8. The lithium iron phosphate fast-charging battery design method according to claim 5, characterized in that, The lithium-ion battery's charge rate C in the correlation model can be adjusted by adjusting one or more of the following: the cumulative percentage of Raman-scanned negative electrode active material reaching 10% and 90% (R10 and R90), the negative electrode coating density (G), the compaction density of the negative electrode sheet after rolling (P), and the electrolyte conductivity (σ). This allows the lithium-ion battery to achieve the desired rate performance.
9. The lithium iron phosphate fast-charging battery design method according to claim 7, characterized in that, When C≥10, lithium-ion batteries have a rate performance of 10C or higher; when 6≤C≤10, lithium-ion batteries have a rate performance of 6C-10C; when 4≤C≤6, lithium-ion batteries have a rate performance of 4C-6C; when C≤4, lithium-ion batteries have a rate performance of less than 4C.
10. The lithium iron phosphate fast-charging battery design method according to claim 4, characterized in that, The negative electrode active material is one or more of artificial graphite and natural graphite.