Method for synergistic leaching of ternary cathode material and nickel-iron alloy

By using a synergistic leaching method of nickel-iron alloy and ternary cathode material of retired lithium-ion batteries, and utilizing elemental nickel, cobalt, and iron in the nickel-iron alloy as reducing agents, the problems of long leaching time and high cost in hydrometallurgical processes are solved, and efficient and low-energy-consumption recovery of valuable metals is achieved.

CN122279226APending Publication Date: 2026-06-26CENT SOUTH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202610544894.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-23
Publication Date
2026-06-26

AI Technical Summary

Technical Problem

Among existing lithium-ion battery recycling technologies, hydrometallurgical processes suffer from high energy consumption, high cost, and severe pollution, and are difficult to industrialize. In particular, the leaching process of nickel-iron alloys and retired lithium-ion battery cathode materials requires the addition of additional reducing agents and oxidizing agents, resulting in long processing times and low efficiency.

Method used

Using elemental nickel, cobalt, and iron from nickel-iron alloys as reducing agents, they are mixed with ternary cathode materials from retired lithium-ion batteries. By controlling the ratio and regulating the reaction conditions, a leaching reaction is carried out in a sulfuric acid solution, without the need to add additional reducing agents or oxidizing agents, to achieve the conversion of high-valence nickel, cobalt, and manganese and the selective precipitation of iron.

Benefits of technology

It achieves a high leaching rate of over 99% for lithium, nickel, cobalt, and manganese, while iron is separated in the form of precipitation, significantly reducing costs and energy consumption, simplifying the process, and making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122279226A_ABST
    Figure CN122279226A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of hydrometallurgical technology, specifically disclosing a method for the co-leaching of ternary cathode materials and nickel-iron alloys. The method provided by this invention includes the following steps: crushing and mixing the nickel-iron alloy and ternary cathode material to obtain a mixture; adding the mixture to a sulfuric acid solution and stirring to leach a reaction; and separating the solid and liquid phases to obtain a leaching solution containing lithium, nickel, cobalt, and manganese, and an iron leaching residue. This invention is the first to propose a method for the co-leaching of ternary cathode materials and nickel-iron alloys from retired lithium-ion batteries. Over 99% of lithium, nickel, cobalt, and manganese are efficiently leached, and over 95% of iron exists as ferric iron precipitate in the leaching residue. This solves the problem of difficult leaching of valuable metals from large-particle nickel-iron alloys and ternary cathode materials, while simultaneously achieving efficient separation of iron from valuable metals such as lithium, cobalt, manganese, and nickel. Furthermore, it saves on the use of reducing agents, oxidizing agents, and pH adjusters, offering advantages such as simple process, low energy consumption, low pollution, and low cost, making it suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hydrometallurgical technology, and in particular to a method for the synergistic leaching of ternary cathode materials and nickel-iron alloys. Background Technology

[0002] Lithium-ion batteries, with their outstanding advantages such as high energy density, long cycle life, low self-discharge rate, and no memory effect, have become a core component of new energy vehicles. Driven by the continued growth in global demand for renewable energy and electric vehicles, the production and consumption of lithium-ion batteries are expanding rapidly. The large-scale development of lithium-ion batteries is highly dependent on a stable supply of key upstream metal materials, whose raw material sources are mainly divided into two categories: primary resources and secondary resources. Primary resources refer to natural mineral resources and intermediate products obtained through mining and metallurgy. Secondary resources refer to valuable materials recovered from waste such as retired lithium-ion batteries, waste alloys, and metallurgical slag. It is worth noting that lithium-ion batteries contain valuable metals such as lithium, nickel, cobalt, and manganese, as well as key components such as separators and electrolytes. Improper disposal of these used batteries can lead to environmental pollution, resource loss, increased waste management pressure, reduced energy security, and exacerbated supply chain risks. Furthermore, battery recycling is a core approach to reducing the environmental impact of battery systems, reducing the consumption of primary mineral resources and alleviating the environmental burden caused by mining, metallurgy, and waste disposal.

[0003] Currently, the mainstream processing technologies for retired lithium-ion batteries are mainly divided into three categories: pyrometallurgy, hydrometallurgy, and direct regeneration. Pyrometallurgy requires high-temperature smelting, resulting in high energy consumption, large carbon dioxide emissions, and high lithium and manganese loss rates, which contradicts the current green development concept. Unlike pyrometallurgy and hydrometallurgy, which primarily extract metal elements from cathode materials, direct regeneration technology aims to regenerate cathode materials while maintaining their structural integrity. This method significantly reduces energy consumption and pollutant emissions during recycling, but it is currently still in the laboratory research stage. Hydrometallurgy, due to its high metal recovery rate, strong selectivity, and flexible production, has become the dominant technology for battery recycling. As a core step in hydrometallurgy, leaching typically requires a reducing agent (such as hydrogen peroxide) or a reducing roasting process to convert the cathode material into a low-valent metal phase. In contrast, when preparing battery-grade nickel sulfate from nickel-iron alloys, H2O2 is usually added as an oxidant to oxidize elemental nickel to divalent nickel, or an oxygen pressure leaching process is used. However, oxygen pressure leaching equipment has stringent requirements and high operational risks.

[0004] Chinese patent CN119101804A proposes adding L-ornithine hydrochloride and ascorbic acid to deionized water and stirring at 40–70°C to generate a colorless and transparent deep eutectic solvent. Waste ternary lithium-ion battery cathode material is then added to the deep eutectic solvent and leached at 40–70°C for 2–8 minutes to obtain a valuable metal leachate. While this method achieves efficient leaching of valuable metals, it involves the high cost and difficulty in reusing the deep eutectic solvent, hindering industrialization. Chinese patent CN115896460A uses ascorbic acid as both a leaching agent and a reducing agent to leach valuable metals from ternary lithium-ion cathode materials. This method involves high-cost organic acids that also act as reducing agents, making industrial application difficult. Chinese patent CN114702079A proposes a method of leaching nickel-iron alloy with sulfuric acid solution, evaporating and concentrating the leachate to obtain a concentrated solution, cooling and crystallizing the concentrated solution, separating the solid and liquid to obtain crude ferrous sulfate crystals and a first solution, adding an oxidant and a phosphorus source to the first solution, adjusting the pH with alkali, heating the reaction, and continuing to adjust the pH of the slurry after the reaction is complete, followed by solid-liquid separation to obtain a nickel sulfate solution and ferric phosphate. This method requires 8-10 hours for the leaching process and necessitates the use of oxidants and pH adjusters to precipitate iron as ferric phosphate. Its limitations in processing efficiency and cost hinder its industrialization. Chinese patent CN114182100A proposes a method of first leaching nickel-iron alloy with sulfuric acid to obtain a mixed solution of nickel sulfate and ferrous sulfate. This mixed solution is then evaporated and crystallized to obtain mixed crystals of nickel sulfate and ferrous sulfate. A certain amount of additives is added to the mixed crystals, and after thorough mixing, the mixture is calcined in a furnace at 500–800°C for 1–5 hours to obtain crystalline clinker. Distilled water is added to the clinker, and the mixture is stirred and dissolved under a water bath heating condition at 25–100°C for 0.5–3 hours. The solution is then filtered to obtain a nickel sulfate solution and iron oxide slag. This method involves a leaching process that takes 8–10 hours and requires the use of oxidants and pH adjusters to precipitate iron as ferric phosphate. The nickel-iron sulfuric acid leaching stage also takes more than 8 hours and requires the addition of salt additives for high-temperature calcination and water leaching to obtain iron oxide slag. This method suffers from drawbacks such as complex processes, long processing times, high costs, and severe pollution.

[0005] Against the backdrop of the rapid development of new energy vehicles, the explosive retirement of lithium-ion batteries, and the continuous growth in demand for lithium, nickel, cobalt, and manganese metals, research on efficient, high-value, and green hydrometallurgical processes for nickel-iron alloys and retired lithium-ion positive materials is imperative. Summary of the Invention

[0006] This invention aims to at least solve one of the technical problems existing in the prior art. To this end, this invention provides a scheme for the co-leaching of nickel-iron alloy and retired ternary lithium-ion battery materials. This invention utilizes elemental nickel, cobalt, and iron in the nickel-iron alloy as reducing agents to convert high-valence nickel, cobalt, and manganese (III / IV) in the ternary cathode material into low-valence (II) states, thereby achieving efficient co-leaching of valuable metals. Simultaneously, by skillfully controlling the ratio of the nickel-iron alloy to the retired ternary cathode material, all iron in the leachate exists in the form of trivalent iron. As the reaction proceeds and the pH of the solution increases, the iron ultimately enters the leaching residue as a precipitate of trivalent iron.

[0007] This invention provides a method for the synergistic leaching of ternary cathode materials and nickel-iron alloys, comprising the following steps:

[0008] S1. The nickel-iron alloy and the ternary cathode material are crushed and mixed to obtain a mixture.

[0009] S2. Add the mixture to a sulfuric acid solution with a concentration of 80~90g / L, and stir and leach at a reaction temperature of 60~90℃.

[0010] S3. After the leaching reaction is completed, solid and liquid are separated to obtain a leaching solution containing lithium, nickel, cobalt and manganese and an iron leaching residue.

[0011] According to specific embodiments of the present invention, the method provided by the present invention can achieve efficient synergistic leaching of valuable metals and precipitation separation of iron elements without adding any additional reducing agents, oxidizing agents, pH adjusters, etc.

[0012] In industrial production, the reaction of nickel-iron alloy with sulfuric acid alone requires more than 8 hours. Adding hydrogen peroxide as an oxidant can shorten the reaction time, but it increases the cost. Similarly, during the leaching process of cathode materials from retired lithium-ion batteries, hydrogen peroxide is usually added as a reducing agent, or reduction roasting is used to convert the high-valence nickel, cobalt, and manganese oxides in the cathode material into low-valence compounds that are easily soluble in acid solutions. This invention innovatively uses elemental Ni, Co, and Fe in nickel-iron alloy as reducing agents to reduce the high-valence Ni, Co, and Mn (III / IV) in ternary cathode materials to low-valence (II) states. At the same time, by precisely controlling the ratio of the two, the iron in the leaching solution is all in the form of Fe. 3+ It exists in the form of Fe, and as the reaction proceeds and the pH increases, it eventually becomes Fe. 3+ The precipitate enters the leaching residue. This invention eliminates the need for adding oxidizing / reducing agents and achieves selective precipitation of iron, significantly reducing reagent costs. It enables efficient, energy-saving, and clean recovery of valuable metals, providing a new pathway for the high-value utilization of secondary resources and demonstrating promising prospects for industrial application.

[0013] According to some embodiments of the present invention, the nickel-iron alloy contains iron, nickel, cobalt and silicon elements; wherein, iron, nickel and cobalt elements are all in the zero valence state.

[0014] According to some embodiments of the present invention, the mass fraction of each element in the nickel-iron alloy is: Fe 50%~60%, Ni 10%~15%, Co 9%~13%, with the balance being Si and impurities.

[0015] According to some embodiments of the present invention, the ternary cathode material is a retired lithium battery ternary cathode material, which includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, or lithium manganese oxide.

[0016] According to some embodiments of the present invention, the D90 particle size after crushing the nickel-iron alloy and the ternary cathode material is ≤500μm.

[0017] The nickel-iron alloy used in this invention mainly uses low-grade laterite nickel ore as the core raw material. It is produced by pyrometallurgical reduction smelting to reduce and fuse nickel, iron and cobalt oxides together, followed by impurity removal, refining and ingot granulation. It has the following characteristics: the raw material is stable and hard, making it difficult to grind. The processing can only be crushed. After crushing, large-particle leaching is used, which is more difficult than leaching ordinary materials.

[0018] According to some embodiments of the present invention, in step S1, the mass ratio of the nickel-iron alloy to the ternary cathode material is (1~1.1):1.

[0019] According to some embodiments of the present invention, in step S2, the concentration of the sulfuric acid solution is 85~90 g / L.

[0020] According to some embodiments of the present invention, in step S2, the ratio of the sulfuric acid solution to the mixture is 8~12 mL / g.

[0021] According to some embodiments of the present invention, in step S2, the leaching reaction time is 80-120 min; during the leaching reaction, stirring is performed at a speed of 300-600 r / min.

[0022] This invention achieves efficient leaching of valuable metals such as lithium, nickel, cobalt, or manganese, and efficient precipitation and separation of iron and silicon elements by precisely controlling the reaction parameters during the leaching process.

[0023] The main reactions that may occur during the leaching reaction in step S2 of the present invention are shown in Table 1 below:

[0024] This invention aims to reveal the leaching mechanism of valuable metals such as lithium, nickel, cobalt, manganese, and iron in retired lithium-ion batteries and nickel-iron alloys. Through thermodynamic calculations (FactSage 8.4), the relationship between the standard Gibbs free energy (ΔG) and temperature for various possible reactions during the synergistic leaching process was systematically studied. It should be noted that the FactSage 8.4 database lacks data on LiNi... x Co y Substances such as Mn2O2, Ni2O3, and Co2O3 are used; therefore, MnO2 and Co3O4 are used to represent high-valence manganese oxides and cobalt oxides in ternary cathode materials. According to the fundamental principles of chemical thermodynamics, the sign and magnitude of the standard Gibbs free energy change (ΔG) can directly determine the spontaneous direction and thermodynamic probability of a chemical reaction. Reactions with ΔG < 0 can proceed spontaneously at a given temperature, while reactions with ΔG > 0 cannot proceed thermodynamically spontaneously.

[0025] Table 1 lists the chemical reaction equations that may occur during the co-leaching process. Figure 1Gibbs free energies were calculated for the possible reactions. The Gibbs free energies for reactions 1-1, 1-2, 1-3, 1-4, 1-8, and 1-9 are all negative and increase with increasing temperature, indicating that heating is unfavorable for these reactions. Meanwhile, the order ΔG(1-2) < ΔG(1-1) < ΔG(1-8) < ΔG(1-3) < ΔG(1-4) < ΔG(1-9) indicates that the co-leaching reaction of elemental Fe with Co3O4 / MnO2 is more likely to occur, while the reaction of elemental Fe, Co3O4, or MnO2 alone with sulfuric acid is more difficult. Furthermore, the relationship ΔG(1-2) < ΔG(1-1) < ΔG(1-23) proves that Fe(0) is first oxidized to Fe(II), and then further oxidized to Fe(III). Similarly, the order ΔG(1-6) < ΔG(1-7) < ΔG(1-5) indicates that elemental nickel can also act as a reducing agent, and the synergistic leaching reaction of elemental nickel with Co3O4 / MnO2 is more likely to occur. The sequence ΔG(1-20) < ΔG(1-21) < ΔG(1-22) indicates that elemental cobalt can act as a reducing agent, and its synergistic leaching with Co3O4 / MnO2 is more likely to occur. The relationship ΔG(1-14) < ΔG(1-15) < ΔG(1-16) indicates that elemental aluminum can act as a reducing agent, and elemental aluminum preferentially undergoes synergistic leaching with Co3O4 / MnO2. The trend ΔG(1-19) < ΔG(1-18) < ΔG(1-17) indicates that elemental copper can act as a reducing agent, and the synergistic leaching reaction of elemental copper with Co3O4 / MnO2 is thermodynamically more likely to occur. Furthermore, the order ΔG(1-13) < ΔG(1-10) < ΔG(1-12) < ΔG(1-11) implies that low-valence metal oxides can react with sulfuric acid, with the preferred order being Li₂O > MnO > CoO > NiO. Additionally, the relationship ΔG(1-14) < ΔG(1-2) < ΔG(1-20) < ΔG(1-6) < ΔG(1-1) < ΔG(1-19) indicates that the reduction order follows Al > Fe(O) > Co > Ni > Fe(II) > Cu.

[0026] Therefore, redox reactions dominate the synergistic leaching process. In this process, elemental Ni, Co, and Fe in the nickel-iron alloy reduce the high-valence Ni, Co, and Mn oxides in the ternary cathode material to lower valence states, thereby achieving efficient leaching of valuable metals Li, Ni, Co, and Mn. Iron initially leaches out as Fe... 2+ The form enters the solution and is gradually oxidized to Fe as the reaction proceeds. 3+ Simultaneously, the pH of the system self-adjusts to 2.5-3.0 during the reaction, promoting Fe... 3+ Ultimately, it enters the leaching residue as a precipitate. The reaction mechanism is as follows: Figure 2 As shown.

[0027] This invention is the first to propose a method for the synergistic leaching of ternary cathode materials and nickel-iron alloys from retired lithium-ion batteries. More than 99% of lithium, nickel, cobalt, and manganese are efficiently leached, and more than 95% of iron exists as ferric iron precipitate in the leaching residue. This solves the problem of difficult leaching solution filtration and achieves efficient separation of silicon, iron, and valuable metals cobalt, copper, and nickel.

[0028] According to some embodiments of the present invention, in step S3, the obtained leachate is purified, extracted, and crystallized to obtain lithium sulfate, nickel sulfate, cobalt sulfate, and / or manganese sulfate.

[0029] This invention targets complex sulfuric acid leachates, which can be subsequently processed using industrially mature extraction separation and precise crystallization methods. The specific steps are as follows: First, deep purification is performed to remove impurity ions such as iron, aluminum, copper, calcium, and magnesium. Then, P204 extraction purification and P507 gradient extraction processes are sequentially used to achieve efficient separation of manganese, cobalt, nickel, and lithium components, yielding high-purity nickel sulfate, cobalt sulfate, manganese sulfate solutions, and enriched lithium sulfate solution, respectively. Finally, through evaporation crystallization and chemical precipitation control, high-purity battery-grade sulfate raw materials and lithium carbonate products are prepared.

[0030] The beneficial effects of this invention are:

[0031] 1) This invention proposes a pure wet leaching process for the first time for this complex large-particle-size nickel-iron alloy and ternary cathode material. Moreover, the recovery index of lithium, nickel, cobalt and manganese can reach more than 99%, and iron exists in the form of precipitate residue with a recovery rate of more than 95%. This achieves efficient and selective separation of iron from other metals such as lithium, nickel, cobalt and manganese.

[0032] 2) This invention solves the problem of long leaching time for processing nickel-iron alloys alone in industry through a wet synergistic leaching process, saving the addition of oxidant (hydrogen peroxide); at the same time, it solves the problem that processing retired lithium-ion cathode materials alone in industry requires the addition of reducing agent (hydrogen peroxide) or pretreatment through reduction roasting; and this invention saves the use of reducing agent, oxidant and pH adjuster, significantly reducing industrialization costs.

[0033] 3) The process of the present invention is simple, energy-efficient, less polluting, and low-cost, which is conducive to industrial production.

[0034] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Attached Figure Description

[0035] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0036] Figure 1This is a graph showing the relationship between the reaction temperature and the standard Gibbs free energy that may occur during the synergistic leaching process of the present invention.

[0037] Figure 2 This is a schematic diagram of the synergistic leaching mechanism of the present invention;

[0038] Figure 3 The image shown is the XRD pattern of the nickel-iron alloy of Example 1 of this invention.

[0039] Figure 4 The image shows the XRD pattern of the ternary cathode material of Embodiment 1 of the present invention.

[0040] Figure 5 This is a laser particle size analysis diagram of the nickel-iron alloy of Example 1 of the present invention;

[0041] Figure 6 This is a laser particle size analysis diagram of the ternary cathode material in Example 1 of the present invention;

[0042] Figure 7 This is a photograph of the iron selective precipitation experiment in Example 1 of the present invention.

[0043] Figure 8 This is a photograph of the leaching residue in Comparative Example 1 of the present invention when there is no iron precipitation. Detailed Implementation

[0044] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.

[0045] Unless otherwise specified in the examples, the procedures should be performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0046] Example 1

[0047] This embodiment provides a method for recovering valuable metals by synergistic leaching of ternary cathode materials from retired lithium batteries and nickel-iron alloys.

[0048] In this embodiment, the nickel-iron alloy primarily uses low-grade laterite nickel ore as its core raw material. It is produced through pyrometallurgical reduction smelting, which reduces and fuses nickel, iron, and cobalt oxides. The alloy is then refined through impurity removal and ingot granulation. The mass fractions of each element are: Fe 56.67%, Ni 12.6%, Co 11.2%, with the remainder being Si and small amounts of impurities. The ternary cathode material for retired lithium batteries is NCM622, with the following valuable metal mass fractions: Mn 11.65%, Fe 0.92%, Co 11.30%, Ni 34.98%, Cu 0.24%, Li 7.04%, Al 0.32%.

[0049] The raw materials were analyzed using XRD. The XRD pattern of the nickel-iron alloy is shown below. Figure 3 As shown, the composition confirms that its phases are mainly elemental iron and Ni-Fe alloy phases. The XRD pattern of the retired lithium-ion battery ternary cathode material is shown below. Figure 4 As shown, it can be seen that the cathode material is mainly composed of ternary compounds (LiNi). x Co y Mn z Composed of O2 and NCM.

[0050] The specific steps of this embodiment are as follows:

[0051] 1) The raw materials were crushed, and the particle size of the crushed raw materials was analyzed by a laser particle size analyzer. The particle size D(90) of the nickel-iron alloy powder was 478.63 μm (e.g., ...). Figure 5 As shown), the particle size D(90) of the ternary cathode material powder is 416.869 μm (as shown). Figure 6 (as shown)

[0052] 2) Mix the nickel-iron alloy powder and the retired lithium battery cathode material powder at a mass ratio of 1:1, and grind them evenly;

[0053] 3) Pour the mixture into a beaker containing a 90 g / L sulfuric acid solution and place it in an 85°C water bath for stirring and leaching. The ratio of sulfuric acid solution to mixture is 10 mL / g, the stirring speed is 500 r / min, and the leaching time is 100 min.

[0054] 4) After leaching for a period of time, the leachate is subjected to solid-liquid separation to obtain leachate and leachate residue.

[0055] Chemical analysis of the leachate revealed that the leaching rates of lithium, nickel, cobalt, and manganese were all above 99%, and 95.1% of the iron existed as precipitate in the leaching residue (e.g., ...). Figure 7 (As shown).

[0056] Example 2

[0057] This embodiment provides a method for recovering valuable metals by synergistic leaching of ternary cathode materials from retired lithium batteries and nickel-iron alloys.

[0058] This embodiment is basically the same as that of Embodiment 1, except that the sulfuric acid concentration in step 3) of this embodiment is 85 g / L, and the rest of the steps are the same as those of Embodiment 1.

[0059] Chemical analysis of the leachate showed that the leaching rates of lithium, nickel, cobalt, and manganese were all above 99%, and 95.26% of the iron existed in the leaching residue as precipitate.

[0060] Example 3

[0061] This embodiment provides a method for recovering valuable metals by synergistic leaching of ternary cathode materials from retired lithium batteries and nickel-iron alloys.

[0062] This embodiment is basically the same as embodiment 1, except that the water bath temperature in step 3) of this embodiment is 80°C, and the other steps are the same as in embodiment 1.

[0063] Chemical analysis of the leachate showed that the leaching rates of lithium, nickel, cobalt, and manganese were all above 99%, and 94.88% of iron existed in the leaching residue as precipitate.

[0064] Example 4

[0065] This embodiment provides a method for recovering valuable metals by synergistic leaching of ternary cathode materials from retired lithium batteries and nickel-iron alloys.

[0066] This embodiment is basically the same as embodiment 1, except that the water bath temperature in step 3) of this embodiment is 60°C, and the other steps are the same as in embodiment 1.

[0067] Chemical analysis of the leachate showed that the leaching rates of lithium, nickel, cobalt, and manganese were all above 99%, and 94.78% of the iron existed in the leaching residue as precipitate.

[0068] Example 5

[0069] This embodiment provides a method for recovering valuable metals by synergistic leaching of ternary cathode materials from retired lithium batteries and nickel-iron alloys.

[0070] This embodiment is basically the same as embodiment 1, except that the leaching time in step 3) of this embodiment is 90 minutes, and the other steps are the same as those in embodiment 1.

[0071] Chemical analysis of the leachate showed that the leaching rates of lithium, nickel, cobalt, and manganese were all above 99%, and 95.01% of the iron existed in the leaching residue as precipitate.

[0072] Example 6

[0073] This embodiment provides a method for recovering valuable metals by synergistic leaching of ternary cathode materials from retired lithium batteries and nickel-iron alloys.

[0074] This embodiment is basically the same as embodiment 1, except that the leaching time in step 3) of this embodiment is 80 minutes, and the other steps are the same as those in embodiment 1.

[0075] Chemical analysis of the leachate showed that the leaching rates of lithium, nickel, cobalt, and manganese were all above 99%, and 94.59% of the iron existed in the leaching residue as precipitate.

[0076] Comparative Example 1

[0077] This comparative example provides a method for recovering valuable metals using synergistic leaching of retired lithium-ion battery ternary cathode materials and nickel-iron alloys.

[0078] This comparative example is basically the same as Example 1, except that in step 2) of this comparative example, the nickel-iron alloy powder and the retired lithium battery cathode material powder are mixed at a mass ratio of 1.2:1. The remaining steps are the same as in Example 1.

[0079] Chemical analysis of the leachate yielded leaching rates of 97.21%, 93.12%, 92.11%, 96.15%, and 92.28% for lithium, nickel, cobalt, manganese, and iron, respectively.

[0080] The actual image of the leaching residue in this comparative example is shown below. Figure 8 As shown.

[0081] Comparative Example 2

[0082] This comparative example provides a method for recovering valuable metals using synergistic leaching of retired lithium-ion battery ternary cathode materials and nickel-iron alloys.

[0083] This comparative example is basically the same as Example 1, except that in step 2) of this comparative example, the nickel-iron alloy powder and the retired lithium battery cathode material powder are mixed at a mass ratio of 0.9:1, and the remaining steps are the same as in Example 1.

[0084] Chemical analysis of the leachate yielded leaching rates of 98.21%, 94.12%, 95.11%, 96.15%, and 94.28% for lithium, nickel, cobalt, manganese, and iron, respectively.

[0085] Comparative Example 3

[0086] This comparative example provides a method for recovering valuable metals using synergistic leaching of retired lithium-ion battery ternary cathode materials and nickel-iron alloys.

[0087] This comparative example is basically the same as Example 1, except that the sulfuric acid concentration in step 3) of this comparative example is 100 g / L, and the other steps are the same as in Example 1.

[0088] Chemical analysis of the leachate revealed that the leaching rates of lithium, nickel, cobalt, manganese, and iron were all above 99%.

[0089] Comparative Example 4

[0090] This comparative example provides a method for recovering valuable metals using synergistic leaching of retired lithium-ion battery ternary cathode materials and nickel-iron alloys.

[0091] This comparative example is basically the same as Example 1, except that the sulfuric acid concentration in step 3) of this comparative example is 80 g / L, and the other steps are the same as those in Example 1.

[0092] Chemical analysis of the leachate revealed that the leaching rates of lithium, nickel, cobalt, and manganese were 95.22%, 93.32%, 94.12%, and 94.12%, respectively, while 87.22% of the iron was present as precipitate in the leachate residue.

[0093] Comparative Example 5

[0094] This comparative example provides a method for recovering valuable metals using synergistic leaching of retired lithium-ion battery ternary cathode materials and nickel-iron alloys.

[0095] This comparative example is basically the same as Example 1, except that the water bath temperature in step 3) of this comparative example is 55°C, and the other steps are the same as in Example 1.

[0096] Chemical analysis of the leachate yielded leaching rates of 96.84%, 96.32%, 96.62%, 96.33%, and 32.1% for lithium, nickel, cobalt, manganese, and iron, respectively.

[0097] Comparative Example 6

[0098] This comparative example provides a method for recovering valuable metals using synergistic leaching of retired lithium-ion battery ternary cathode materials and nickel-iron alloys.

[0099] This comparative example is basically the same as Example 1, except that the leaching time in step 3) of this comparative example is 75 min, and the other steps are the same as those in Example 1.

[0100] Chemical analysis of the leachate revealed that the leaching rates of lithium, nickel, cobalt, and manganese were 96.82%, 96.42%, 96.57%, and 96.43%, respectively, while 90.1% of the iron was present as precipitate in the leachate residue.

[0101] In summary, the technical solution of this invention proposes a pure wet leaching process for complex, large-particle-size nickel-iron alloys and ternary cathode materials, achieving efficient and selective separation of iron from other metals such as lithium, nickel, cobalt, and manganese. Furthermore, the process of this invention solves the problem of long leaching time for nickel-iron alloys in industrial processing, saves the use of additional reagents such as oxidants, reducing agents, and pH adjusters, and eliminates the need for high-energy-consuming processes such as calcination. It has the advantages of low cost, low energy consumption, and low pollution, making it suitable for industrial production.

[0102] In Comparative Example 1, excessive use of nickel-iron alloy leads to the consumption of sulfuric acid in the solution by its valuable metals. This results in the acid in the system failing to fully leach the valuable metals from the ternary material and the nickel-iron alloy. Simultaneously, since elemental iron is preferentially oxidized to ferrous iron, a high nickel-iron content hinders the further oxidation of ferrous iron to ferric iron by the high-valence nickel, cobalt, and manganese in the ternary cathode material. This prevents iron from precipitating and affects the selective separation of iron. In Comparative Example 2, insufficient use of nickel-iron alloy fails to adequately reduce the high-valence nickel, cobalt, and manganese in the ternary cathode material to lower valence states, resulting in insufficient leaching of valuable metals. Furthermore, insufficient nickel-iron alloy also leads to excessively high solution acidity, thus affecting the selective precipitation of ferric iron.

[0103] In Comparative Examples 3 and 4, the concentration of sulfuric acid in the leaching solution was adjusted to be too high and too low, respectively. If the acidity was too high, iron would also exist in the leaching solution in the form of ions. If the acidity was too low, the nickel-iron alloy and the ternary cathode material could not achieve a full synergistic reaction, making it difficult to achieve efficient and selective separation of iron from other metals.

[0104] In Comparative Example 5, the leaching temperature was too low, resulting in a slow synergistic reaction rate. After a certain reaction time, the valuable metals in the nickel-iron alloy and the ternary cathode material could not be fully leached, leading to a high residual acid content in the solution. Ultimately, this resulted in the inability of ferric iron to precipitate effectively, thus failing to achieve selective separation of iron from valuable metals.

[0105] In Comparative Example 6, the leaching reaction time was too short, and the valuable metals in the nickel-iron alloy and ternary cathode material could not be fully leached. At the same time, the acidity in the solution was too high, which prevented the ferric iron from precipitating sufficiently, thus failing to achieve efficient and selective separation of iron and valuable metals.

[0106] The embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof can be combined with each other unless otherwise specified.

Claims

1. A method for the synergistic leaching of ternary cathode material and nickel-iron alloy, characterized in that, Includes the following steps: S1. The nickel-iron alloy and the ternary cathode material are crushed and mixed to obtain a mixture. S2. Add the mixture to a sulfuric acid solution with a concentration of 80~90g / L, and stir and leach at a reaction temperature of 60~90℃. S3. After the leaching reaction is completed, solid and liquid are separated to obtain a leaching solution containing lithium, nickel, cobalt and / or manganese and an iron leaching residue.

2. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 1, characterized in that, The nickel-iron alloy contains iron, nickel, cobalt and silicon; wherein iron, nickel and cobalt are all in the zero valence state.

3. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 2, characterized in that, The nickel-iron alloy contains the following mass fractions of elements: Fe 50%~60%, Ni 10%~15%, Co 9%~13%, with the balance being Si and impurities.

4. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 1, characterized in that, The ternary cathode material is a retired lithium battery ternary cathode material, which includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, or lithium manganese oxide.

5. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 1, characterized in that, The D90 particle size after crushing the nickel-iron alloy and ternary cathode material is ≤500μm.

6. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 1, characterized in that, In step S1, the mass ratio of the nickel-iron alloy to the ternary cathode material is (1~1.1):

1.

7. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 1, characterized in that, In step S2, the concentration of the sulfuric acid solution is 85~90g / L, and the ratio of the sulfuric acid solution to the mixture is 8~12mL / g.

8. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 1, characterized in that, In step S2, the leaching reaction takes 80-120 minutes; during the leaching reaction, the mixture is stirred at a speed of 300-600 r / min.

9. The method for synergistic leaching of ternary cathode material and nickel-iron alloy according to claim 1, characterized in that, In step S3, the obtained leachate is purified, extracted, and crystallized to obtain lithium sulfate, nickel sulfate, cobalt sulfate, and / or manganese sulfate.

Citation Information

Patent Citations

  • Method for efficiently separating nickel and iron from nickel-iron alloy

    CN114182100A

  • Method for separating and extracting nickel and iron from nickel-iron alloy

    CN114702079A

  • Method for synergistically leaching manganese, cobalt, nickel and lithium from waste ternary lithium ion battery positive electrode material

    CN115896460A

  • Method for leaching valuable metal from waste ternary lithium ion battery positive electrode material NCM111

    CN119101804A