Water-barrier laminated film
By setting an isocyanate-based coating between the moisture-capturing layer and the inorganic barrier layer, the problem of poor adhesion between the moisture-capturing layer and the inorganic barrier layer is solved, achieving high adhesion and stable moisture barrier properties, thereby improving production efficiency.
Patent Information
- Application Number
- CN202610371468.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-11-07
- Filing Date
- 2018-11-07
- Publication Date
- 2026-07-03
AI Technical Summary
In the prior art, the adhesion between the moisture-capturing layer and the inorganic barrier layer is poor, which makes it easy to crack and peel off during heating and drying, affecting the moisture barrier properties and the appearance of the film. Furthermore, prolonged heating at high temperatures can cause the plastic film to deform.
An isocyanate-based coating is placed between an inorganic barrier layer and a moisture-capturing layer. The polymer generated by the isocyanate reaction is used as the film-forming component, especially a high-Tg urethane resin and a cross-linked structure, to form an isocyanate-based coating as a base layer, thereby improving adhesion.
It effectively prevents the moisture-capturing layer from cracking, maintains high adhesion, avoids peeling, improves productivity, ensures moisture barrier properties and membrane stability, and avoids the adverse effects of prolonged high-temperature heating.
Smart Images

Figure CN122325819A_ABST
Abstract
Description
[0001] This application is a divisional application of the application filed on November 7, 2018, with application number 201880072107.3 and invention title "Moisture-Barrier Laminate". Technical Field
[0002] This invention relates to a moisture-barrier laminate having an inorganic barrier layer and a moisture-capturing layer. The invention further relates to a coating composition for forming a substrate layer of the moisture-capturing layer. Background Technology
[0003] As a means of improving the properties of various plastic substrates, especially their gas barrier properties, a technique is known to form an inorganic thin film (inorganic barrier layer) such as silicon oxide by vacuum evaporation on the surface of the plastic substrate (Patent Document 1). Films with such inorganic thin films are widely used as barrier films.
[0004] Various electronic devices developed and put into practical use in recent years, such as organic electroluminescent (organic EL) devices, solar cells, touch panels, and electronic paper, require high moisture barrier properties. In order to meet the above requirements, the applicant has proposed a moisture barrier laminate with a moisture-capturing layer laminated thereon (Patent Document 2).
[0005] The aforementioned moisture-capturing layer is formed by coating a moisture-capturing layer composition onto an inorganic barrier layer formed on the surface of a plastic film by means of vacuum evaporation, and then curing the coating composition.
[0006] However, when a moisture-capturing layer is formed by directly coating the coating composition onto the inorganic barrier layer as described above, there is a problem that the moisture-capturing layer itself undergoes cracking due to volume shrinkage during heating and drying, resulting in a deterioration of both moisture barrier properties and the appearance of the film. Furthermore, the adhesion between the inorganic barrier layer and the moisture-capturing layer is weak, therefore, the film is prone to delamination due to volume expansion during moisture absorption.
[0007] The adhesion between the water-trapping layer and the inorganic barrier layer can be improved, for example, by heating at 100°C for more than one hour after the water-trapping layer has been formed. However, prolonged heating at high temperatures is not only very detrimental to productivity but also causes deformation of the plastic film beneath the inorganic barrier layer and may promote cracking in the formed water-trapping layer. Therefore, it is desirable to improve the adhesion between the water-trapping layer and the inorganic barrier layer without prolonged heating at high temperatures.
[0008] However, to date, there has been no in-depth study on the adhesion between the moisture trapping layer and the inorganic barrier layer in relation to short-term heating of the moisture trapping layer at 100°C. Existing technology
[0009] Patent documents:
[0010] Patent Document 1: Japanese Patent Application Publication No. 2000-255579
[0011] Patent Document 2: Japanese Patent Application Publication No. 2015-96320 Summary of the Invention
[0012] The problem the invention aims to solve
[0013] Therefore, one object of the present invention is to provide a moisture-barrier laminate comprising a plastic film (A) having an inorganic barrier layer (A1) on its surface and a moisture-capturing layer (B), wherein the plastic film (A) and the moisture-capturing layer (B) have excellent adhesion to each other.
[0014] Another object of the present invention is to provide a coating composition for forming a layer located below a moisture-capturing layer.
[0015] Solution for solving the problem
[0016] According to the present invention, a moisture-barrier laminate comprising a plastic film (A) having an inorganic barrier layer (A1) on its surface and a moisture-capturing layer (B) is provided, characterized in that,
[0017] Between the inorganic barrier layer (A1) and the moisture-capturing layer (B), an isocyanate-based coating (C) is provided, containing an isocyanate-based polymer obtained by reacting an isocyanate as a reactive component, as a film-forming component; and
[0018] The moisture-capturing layer (B) is formed on the isocyanate-based coating (C) which serves as the base layer.
[0019] The following embodiments are preferred in the moisture-barrier laminate of the present invention.
[0020] (1) The isocyanate polymer is polyurethane.
[0021] (2) The polyurethane is a high Tg urethane resin with a glass transition point of 60°C or higher.
[0022] (3) The weight-average molecular weight (Mw) of the high Tg urethane resin is above 14,000.
[0023] (4) The polyurethane has a crosslinking structure introduced therein due to at least one functional group selected from the group consisting of epoxy groups, silanol groups and isocyanate groups.
[0024] (5) The isocyanate polymer is a polymer obtained by curing an isocyanate reactive resin with a polyisocyanate.
[0025] (6) The isocyanate reactive resin is a (meth)acrylic resin or a polyester resin.
[0026] (7) The isocyanate reactive resin is a high Tg resin with a glass transition point of 60°C or higher.
[0027] (8) The weight-average molecular weight (Mw) of the high Tg resin is 14,000 or more.
[0028] (9) The moisture-capturing layer (B) contains a hygroscopic polymer.
[0029] (10) The moisture-capturing layer (B) has a structure in which a desiccant with a lower ultimate humidity than the matrix is dispersed in a hygroscopic matrix of an ionic polymer.
[0030] (11) The ionic polymer contained in the moisture-capturing layer (B) is a cationic polymer.
[0031] (12) A protective layer (D) is provided between the inorganic barrier layer (A1) and the isocyanate coating (C).
[0032] (13) The protective layer (D) contains a water-soluble polymer component (D1) and at least one component (D2) selected from the group consisting of organoalkoxysilanes or their hydrolysis products, metal alkoxides or their hydrolysis products, and phosphorus compounds.
[0033] The moisture-barrier laminate of the present invention can be advantageously used as a sealing material for electronic devices.
[0034] Furthermore, according to the present invention, a coating composition for forming a base layer of a moisture-capturing layer is provided, the coating composition being obtained by dissolving or dispersing urethane resin particles in a solvent, characterized in that the solvent contains a curing agent dissolved or dispersed therein having at least one functional group selected from the group consisting of epoxy groups, silanol groups and isocyanate groups.
[0035] In the coating composition, it is desirable that
[0036] (1) The urethane resin particles are high Tg polyurethane with a glass transition point of 60°C or higher.
[0037] (2) The urethane resin particles are formed from urethane polymers with a weight-average molecular weight (Mw) of 14,000 or more.
[0038] (3) The urethane resin particles have a particle size of 0.02 to 3 μm;
[0039] (4) As the curing agent, the polyisocyanate is contained in an amount of 1 to 50 parts by weight relative to 100 parts by weight of the urethane resin particles; and
[0040] (5) As the curing agent, the silane coupling agent is contained in an amount of 0.1 to 50 parts by weight relative to 100 parts by weight of the urethane resin particles.
[0041] According to the present invention, a coating composition for forming a base layer of a moisture-capturing layer is provided, the coating composition being obtained by dissolving or dispersing isocyanate reactive resin particles in a solvent, characterized in that the solvent contains a polyisocyanate dissolved or dispersed therein as a curing agent.
[0042] In the coating composition, it is desirable that,
[0043] (1) The isocyanate reactive resin is a (meth)acrylic resin or a polyester resin;
[0044] (2) The isocyanate reactive resin is a high Tg resin with a glass transition point above 60°C; and
[0045] (3) The weight-average molecular weight (Mw) of the high Tg resin is above 14,000.
[0046] The effects of the invention
[0047] The moisture-barrier laminate of the present invention has a basic structure in which a moisture-capturing layer (B) is provided on an inorganic barrier layer (A1) present on the surface of a plastic film (A). Here, an important feature is that an isocyanate-based coating (C) is present between the moisture-capturing layer and the inorganic barrier layer, located below the moisture-capturing layer. That is, the isocyanate-based coating (C) contains a polymer (typically polyurethane) obtained by reacting isocyanate as a reactive component as a film-forming component (matrix). In the present invention, the moisture-capturing layer is formed on the isocyanate-based coating (C) as a base layer, effectively mitigating the stress generated in the moisture-capturing layer during heat drying. As a result, cracking of the moisture-capturing layer is effectively prevented.
[0048] Furthermore, in this invention, the composition of the isocyanate-based coating (C) is adjusted to greatly improve the adhesion to the moisture-trapping layer (B). For example, as shown in the experimental examples described later, when the moisture-trapping layer forming coating composition is directly applied to the surface of the inorganic barrier layer without forming the isocyanate-based coating (C) as a base layer, the adhesion is about 0.2 N / 15 mm.
[0049] On the other hand, according to the present invention, an isocyanate-based coating (C) (e.g., a urethane-based coating) is formed on the surface of the inorganic barrier layer below the moisture-trapping layer (B). In this case, the moisture-trapping layer formed by heating under the exact same conditions as those described above exhibits improved adhesive strength. In particular, when the crosslinking structure is introduced with functional groups of any one of epoxy, silanol, or isocyanate groups, the adhesive strength is greatly improved to about 1 N / 15 mm.
[0050] As described above, the moisture-capturing layer (B) with improved adhesion can be firmly held on the inorganic barrier layer via the isocyanate-based coating (C) and can effectively prevent peeling.
[0051] As described above, the moisture-barrier laminate according to the present invention effectively prevents breakage of the moisture-trapping layer (B) and fully utilizes its performance, i.e., exhibits excellent moisture barrier properties. Furthermore, the moisture-trapping layer (B) maintains high adhesion even without prolonged heat treatment at temperatures above 100°C. Therefore, improved productivity can be ensured, thus providing significant advantages in an industrial sense. Attached Figure Description
[0052] [ Figure 1 [This is a schematic diagram of an example of the layer structure of the moisture-barrier laminate of the present invention.]
[0053] [ Figure 2 For in Figure 1 A schematic diagram of the structure of the moisture-capturing layer (B) in a moisture-barrier laminate.
[0054] [ Figure 3 This is a schematic diagram of another layer structure of a moisture-barrier laminate. Detailed Implementation
[0055] exist Figure 1 In the present invention, the moisture-barrier laminate, generally designated as 10, has a plastic film (A) as a substrate. An inorganic barrier layer (A1) is formed on the surface of the plastic film (A). On the inorganic barrier layer (A1), an isocyanate-based coating (C) is formed as a base layer for a moisture-capturing layer (B). That is, the isocyanate-based coating (C) and the moisture-capturing layer (B) are sequentially formed on the inorganic barrier layer (A1) on the surface of the plastic film (A).
[0056] Furthermore, the plastic film (A) may have a protective layer (D) formed on the inorganic barrier layer (A1). That is, the isocyanate-based coating (C) may be directly laminated onto the inorganic barrier layer (A1), or as... Figure 3 As shown, it can be laminated onto a protective layer (D) that is appropriately disposed on an inorganic barrier layer (A1).
[0057] <Plastic film (A)>
[0058] The membrane (A) is located below the inorganic barrier layer (A1) and is typically formed using thermoplastic or thermosetting resins, depending on its morphology, based on methods such as injection or co-injection molding, extrusion or co-extrusion molding, film or sheet forming, compression molding, or casting polymerization.
[0059] Generally, from the perspective of formability and cost, films are formed using thermoplastic resins.
[0060] Examples of thermoplastic resins include low-density polyethylene, high-density polyethylene, polypropylene, poly(1-butene), poly(4-methyl-1-pentene), or random or block copolymers of α-olefins such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene; ethylene-vinyl compound copolymers such as ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, and ethylene-vinyl chloride copolymers; styrene-based resins such as polystyrene, acrylonitrile-styrene copolymers, ABS, and α-methylstyrene-styrene copolymers; and polyvinyl chloride, polyvinylidene chloride, and vinyl chloride-vinylidene chloride copolymers. Polyvinyl chloride copolymers, polymethyl acrylate, and polymethyl methacrylate, etc.; polyamides such as nylon 6, nylon 6-6, nylon 6-10, nylon 11, and nylon 12; thermoplastic polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate (PEN); polycarbonate; polyphenylene ether; and biodegradable resins such as polyimide resins, polyamide-imide resins, polyether-imide resins, fluorinated resins, allyl resins, polyurethane resins, cellulose resins, polysulfone resins, polyethersulfone resins, ketone resins, amino resins, and polylactic acid. Furthermore, blends thereof, or resins appropriately modified by copolymerization (e.g., acid-modified olefin resins, etc.), can be used.
[0061] The plastic film (A) is preferably formed from a gas barrier resin with excellent oxygen barrier properties, such as an ethylene-vinyl alcohol copolymer, and may further have a multilayer structure including layers formed by using such a gas barrier resin.
[0062] In this invention, from the viewpoints of availability, cost, formability, partial oxygen barrier properties, and suitability for formation beneath the inorganic barrier layer (A1) as described later, the plastic film (A) is preferably made of a polyester resin represented by polyethylene terephthalate (PET) or an olefin resin represented by polyethylene or polypropylene.
[0063] There are no particular restrictions on the thickness of the plastic film (A), and its thickness can be appropriately determined according to the application.
[0064] <Inorganic barrier layer (A1)>
[0065] The inorganic barrier layer (A1) formed on the surface of the plastic film (A) can be one known per se, for example, as disclosed in Japanese Patent Application Publication No. 2015-96320. That is, the inorganic barrier layer (A1) can be a film formed by physical deposition, represented by vacuum evaporation or ion plating, or it can be an inorganic film formed by chemical deposition, represented by plasma CVD, i.e., a film formed by depositing metal or metal oxides, to ensure high oxygen barrier properties. In particular, from the viewpoint of uniformly forming a film even on an uneven surface and exhibiting excellent barrier properties against moisture and oxygen, it is desirable to form the inorganic barrier layer (A1) on the plastic film (A) serving as the substrate layer by plasma CVD.
[0066] To deposit a film by plasma CVD, a plastic film (A) serving as a substrate layer (A1) is placed in a plasma processing chamber maintained at a predetermined vacuum level. A gas for film formation (reactant gas) containing a metal or metal-containing compound, along with an oxidizing gas (typically oxygen or NOx gas) and a suitable carrier gas such as argon or helium, is then supplied via a gas supply pipe to the plasma processing chamber, which is shielded by a metal wall and wherein the vacuum level is reduced to the predetermined vacuum level. In this state, a glow discharge is generated using a microwave or high-frequency electric field, and plasma is generated by its electrical energy. The decomposition reaction products of the aforementioned compound are deposited on the surface of the plastic film A to form the film.
[0067] As the aforementioned reactant gas, from the viewpoint of forming a membrane at the interface with the substrate membrane (A) having a soft region containing carbon and further having a region with high oxidation degree and excellent barrier properties, it is generally desirable to use gases such as organoaluminum compounds like trialkylaluminum, or organotitanium compounds, organozirconium compounds, or organosilicon compounds. In particular, from the viewpoint of relatively easily and efficiently forming an inorganic barrier layer (A1) with high oxygen barrier properties, organosilicon compounds are most desirable.
[0068] As organosilicon compounds, organosilicon compounds such as hexamethyldisilane, vinyltrimethylsilane, methylsilane, dimethylsilane, trimethylsilane, diethylsilane, propylsilane, phenylsilane, methyltriethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, phenyltrimethoxysilane, methyltrimethoxysilane, and methyltriethoxysilane can be used; as well as organosilicon compounds such as octamethylcyclotetrasiloxane, 1,1,3,3-tetramethyldisiloxane, and hexamethyldisiloxane can also be used. In addition, aminosilanes and silazanes can be used.
[0069] The aforementioned organometallic compounds can be used alone or in combination of two or more.
[0070] The thickness of the inorganic barrier layer (A1) can vary depending on the application of the moisture barrier laminate and the required level of barrier properties. However, generally, the inorganic barrier layer (A1) should be selected to ensure a water vapor permeability of 10. -1 g / m 2 • Below the level of atom, especially 10 -2 g / m 2 • A thickness of less than one day / atom without impairing the properties of the plastic film (A) deposited thereon. Although varying depending on the proportion occupied by the aforementioned high-oxidation regions, the inorganic barrier layer (A1) should typically have a thickness of 4 to 500 nm, particularly about 30 to about 400 nm.
[0071] The aforementioned inorganic barrier layer (A1) can also be formed on the plastic film (A) by methods such as coating instead of vacuum evaporation. That is, the inorganic barrier layer (A1) formed by coating can have lower properties, such as oxygen barrier properties, than the inorganic barrier layer formed by vacuum evaporation. However, depending on the required degree of barrier properties against gases such as oxygen, the inorganic barrier layer (A1) can be a layer formed by coating.
[0072] When using a coating method, the inorganic barrier layer (A1) can be typically formed by coating a solution of an organic solvent containing a polysilazane, a condensation-promoting silane compound (e.g., siloxysilane), and an inorganic fine-particle material suitable for mixing with, for example, silica or alumina, onto a predetermined surface. Subsequently, the organic solvent solution is heated, and the organic solvent is evaporated, thereby forming a film.
[0073] <Moisture-trapping layer (B)>
[0074] The moisture-trapping layer (B) is used to block moisture flowing along the thickness direction of the moisture-barrier laminate 10. There are no particular limitations on the moisture-trapping layer (B), provided that it exhibits moisture-blocking properties. The moisture-trapping layer (B) can be a layer known per se, for example, a layer formed by dispersing a physical desiccant such as zeolite or silica gel in a predetermined resin layer, a layer formed by dispersing a chemical desiccant such as calcium oxide in a predetermined resin layer, or a layer formed by using a hygroscopic nonionic polymer such as polyvinyl alcohol, water-soluble nylon, or polyethylene oxide.
[0075] When a particularly high level of moisture barrier properties is required, it is desirable to form the layer using, for example, an ionic polymer disclosed in Japanese Patent Application Publication No. 2015-96320 as the matrix, and dispersing a desiccant with a lower moisture content than the ionic polymer within the matrix. When such an ionic polymer is used as the matrix, the moisture-trapping layer exhibits excellent moisture-trapping properties. Furthermore, moisture can be confined within the dispersed desiccant. This effectively prevents deformation, such as swelling, caused by moisture absorption.
[0076] Ionic polymers;
[0077] The ionic polymer used in this invention can be a cationic polymer or anionic polymer as described below.
[0078] Cationic polymers are polymers whose molecules contain cationic groups that can become positively charged in water, such as amino to tertiary amino groups, quaternary ammonium groups, pyridyl groups, imidazole groups, or quaternary pyridinium groups. Cationic polymers can form hygroscopic matrices due to the strong nucleophilic interaction of their cationic groups and their ability to capture moisture through hydrogen bonds.
[0079] Generally, the amount of cationic groups in cationic polymers is such that the water absorption rate of the formed hygroscopic matrix at 80% RH and 30°C (JIS K-7209-1984) is more than 5%, and particularly 30% to 45%.
[0080] As a cationic polymer, a cationic polymer is used by suitably polymerizing or copolymerizing at least one of cationic monomers represented by amine monomers such as allylamine, ethyleneimine, vinylbenzyltrimethylamine, [4-(4-vinylphenyl)-methyl]-trimethylamine, or vinylbenzyltriethylamine; nitrogen-containing heterocyclic monomers such as vinylpyridine or vinylimidazole; or their salts, with other copolymerizable monomers, and then further neutralizing them partially by acid treatment as needed.
[0081] Cationic polymers have been described in detail, for example, in Japanese Patent Application Publication No. 2015-96320, and therefore will not be described in detail here. However, generally speaking, from the viewpoint of film-forming properties, polyallylamine is preferred.
[0082] On the other hand, anionic polymers are polymers whose molecules contain anionic functional groups that can become negatively charged in water, such as carboxylic acid groups, sulfonic acid groups, or phosphonic acid groups, or partially neutralized acidic bases. Anionic polymers with such functional groups can form hygroscopic matrices because these functional groups capture water through hydrogen bonding.
[0083] The amount of anionic groups in anionic polymers can vary depending on the type of functional groups, but it is generally intended to make the water absorption rate of the formed hygroscopic matrix at 80% RH and 30°C (JIS K-7209-1984) greater than 5%, and particularly 30% to 45%.
[0084] An anionic polymer having the above functional groups is obtained by polymerizing or copolymerizing at least one of the following anionic monomers: carboxylic acid monomers such as methacrylic acid, acrylic acid, and maleic anhydride; sulfonic acid monomers such as α-halovinylsulfonic acid, styrene sulfonic acid, and vinyl sulfonic acid; phosphonic acid monomers such as vinyl phosphoric acid; or salts thereof, with other monomers that can be copolymerized therewith, followed by partial neutralization with an alkali as needed.
[0085] Anionic polymers have been described in detail, for example, in Japanese Patent Application Publication No. 2015-96320, and therefore will not be described in detail here. However, in general, poly(meth)acrylic acid and its partially neutralized products (e.g., in which a portion is a sodium salt) can be used.
[0086] The structure of the moisture trapping layer (B);
[0087] Reference Figure 2 (a) or (b), it is desirable to blend the moisture-trapping layer (B) with a desiccant that has a lower reach of humidity than the ionic polymer (cationic or anionic polymer) that forms the matrix.
[0088] When a hygroscopic agent with higher hygroscopicity than the matrix is dispersed, the moisture absorbed by the matrix of the ionic polymer can now be easily captured by the hygroscopic agent and effectively confined within the matrix. Therefore, even in very low humidity atmospheres, the moisture-trapping layer (B) effectively exhibits its moisture-trapping capacity. Furthermore, despite absorbing moisture, the moisture-trapping layer (B) effectively inhibits swelling.
[0089] As highly hygroscopic desiccants, those with a reach humidity of 6% or less in an environment with 80% RH and a temperature of 30°C are preferred, provided that they have a lower reach humidity than ionic polymers. If the reach humidity of the desiccant is higher than that of the ionic polymer, the moisture absorbed through the matrix cannot be adequately contained and tends to be released, and a significant improvement in moisture barrier properties cannot be expected. Furthermore, even if the reach humidity is lower than that of the ionic polymer, if the reach humidity measured under the above conditions is higher than the above range, moisture in a low-humidity atmosphere cannot be adequately captured. In this case, moisture barrier properties are often not sufficiently demonstrated.
[0090] The above-mentioned desiccants generally have a water absorption rate of over 50% under an environment of 80% RH humidity and 30℃ temperature (JIS K-7209-1984), and are either inorganic or organic.
[0091] Examples of inorganic hygroscopic agents include clay minerals such as zeolite, alumina, activated carbon, and montmorillonite, as well as silica gel, calcium oxide, and magnesium sulfate.
[0092] Examples of organic desiccant include crosslinked products of anionic polymers or partially neutralized products thereof. Examples of anionic polymers include polymers obtained by polymerizing or copolymerizing at least one of anionic monomers represented by carboxylic acid monomers ((meth)acrylic acid, anhydrous maleic acid, etc.), sulfonic acid monomers (halovinyl sulfonic acid, styrene sulfonic acid, vinyl sulfonic acid, etc.), phosphonic acid monomers (vinyl phosphoric acid, etc.), or salts of their monomers. Organic desiccant is particularly effective in applications requiring transparency. For example, fine particles of crosslinked sodium (meth)acrylate can be representatively used as organic desiccant.
[0093] In this invention, from the viewpoint of exhibiting a large specific surface area and high hygroscopicity, it is desirable to use hygroscopic agents with small particle size (e.g., an average primary particle size of 100 nm or less, particularly 80 nm or less), and most desirable are hygroscopic agents based on organic polymers with small particle size.
[0094] That is, the organic polymer hygroscopic agent is very well dispersed in the ionic polymer matrix, i.e., uniformly dispersed. Furthermore, by employing emulsion polymerization or suspension polymerization as the polymerization method for manufacturing it, hygroscopic agents with fine and uniform spherical particle shapes can be obtained. By adding a certain amount or more of the organic polymer hygroscopic agent, high transparency can be ensured.
[0095] Furthermore, as mentioned above, organic micro-desiccants exhibit very low humidity levels, high hygroscopicity, and minimal volume change despite swelling due to cross-linking. Therefore, organic micro-desiccants are best suited for maintaining an absolutely dry or near-absolutely dry environment while suppressing volume change.
[0096] As an organic desiccant, fine particles can be placed in a commercially available cross-linked polyacrylic acid Na fine particle (average particle size of about 70 nm) in the form of a colloidal dispersion (pH=10.4) from Toyobo Co. under the trade name TAFTIC HU-820E.
[0097] In this invention, from the viewpoint of fully exhibiting its properties, greatly improving moisture barrier properties, effectively suppressing dimensional changes caused by swelling, and ensuring that the moisture barrier properties are higher than those of the inorganic barrier layer (A1) over a long period of time, the amount of desiccant is set according to the type of ionic polymer.
[0098] For example, in applications requiring particularly high moisture barrier properties, the moisture trapping layer (B) is sufficient to exhibit a water vapor permeability of 10. -5 g / m 2 A high-barrier thickness (e.g., 1 μm or more, particularly about 2 to about 20 μm) is formed. However, when the matrix is formed of a cationic polymer, it is desirable to use a desiccant in an amount of 50 parts by weight or more relative to 100 parts by weight of the ionic polymer in the moisture-trapping layer (B), particularly in an amount of 100 to 900 parts by weight, and more preferably in an amount of 200 to 600 parts by weight. Furthermore, when the matrix is formed of anionic polymer, it is desirable to use a desiccant in an amount of 50 parts by weight or more relative to 100 parts by weight of the anionic polymer in the moisture-trapping layer B, particularly in an amount of 100 to 1300 parts by weight, and more preferably in an amount of 150 to 1200 parts by weight.
[0099] In the water-trapping layer (B) having the structure described above, it is desirable for the ionic polymer to have a cross-linked structure introduced therein. That is, when the ionic polymer with the cross-linked structure absorbs water, the molecules of the cationic polymer are bound together by cross-linking. Therefore, the water-trapping layer (B) suppresses its volume change caused by swelling (water absorption) and increases mechanical strength and dimensional stability.
[0100] A cross-linking structure can be introduced by adding a cross-linking agent to the coating composition that forms the moisture-trapping layer (B). In particular, in the case of anionic polymers, unlike cationic polymers, moisture is trapped solely by hydrogen bonds. Therefore, hygroscopicity can be greatly improved by introducing a spatial network structure (cross-linking structure) suitable for moisture absorption into the matrix.
[0101] The crosslinking agents used to introduce the crosslinking structure differ slightly depending on whether the crosslinking structure is introduced into a cationic polymer or an anionic polymer.
[0102] As crosslinking agents for cationic polymers, compounds having crosslinking functional groups (e.g., epoxy groups) capable of reacting with cationic groups and functional groups (e.g., alkoxysilane groups) capable of forming siloxane structures in the crosslinked structure via hydrolysis and dehydration / condensation can be used. In particular, silane compounds represented by the following formula (1) are preferred:
[0103] X–SiR 1n (OR 2 ) 3-n (1)
[0104] Where X is an organic group with an epoxy group at the end.
[0105] R 1 and R 2 They are methyl, ethyl, or isopropyl, respectively, and
[0106] n is 0, 1, or 2.
[0107] Silane compounds have epoxy and alkoxysilyl groups as functional groups. The epoxy group undergoes an addition reaction with the functional group (e.g., NH2) of the cationic polymer. On the other hand, the alkoxysilyl group is hydrolyzed to generate a silanol group (SiOH group), and grows by forming a siloxane structure via its condensation reaction, ultimately forming a cross-linked structure between the cationic polymer chains. Therefore, the matrix of the cationic polymer has a cross-linked structure with a siloxane structure introduced therein.
[0108] Furthermore, the cationic polymer is alkaline. As a result, when a moisture-trapping layer B is formed by coating a composition containing a cationic polymer, the addition reaction between cationic groups and epoxy groups is rapidly promoted, as is the dehydration condensation between silanol groups, and cross-linking structures can be readily introduced.
[0109] In this invention, γ-epoxypropoxyalkylene can be used as the organic group X having an epoxy group in formula (1) above. For example, γ-epoxypropoxypropyltrimethoxysilane or γ-epoxypropoxypropylmethyldimethoxysilane are preferably used as crosslinking agents.
[0110] As a crosslinking agent, a crosslinking agent with an alicyclic epoxy group, such as epoxycyclohexyl, in formula (1) above can also be used. For example, when a compound having an alicyclic epoxy group, such as β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, is used as a crosslinking agent, the alicyclic structure can be introduced into the crosslinking structure of the matrix together with the siloxane structure. The introduction of the alicyclic structure makes it possible to more effectively demonstrate the function of the matrix for forming a hygroscopic spatial network structure.
[0111] Furthermore, in order to introduce the alicyclic structure into the above-mentioned crosslinking structure, compounds having multiple epoxy groups and alicyclic groups are permitted to be used, for example, diglycidyl esters represented by the following formula (2) as crosslinking agents:
[0112] GO(C=O)-A-(C=O)OG(2)
[0113] Wherein, G is a glycidyl group, and
[0114] A is a divalent hydrocarbon group with an aliphatic ring, such as a cycloalkylene group.
[0115] A representative example of diglycidyl ester is represented by the following formula (2-1).
[0116] [Chemical Formula 1]
[0117] (2-1)
[0118] The diglycidyl ester of formula (2) does not have an alkoxysilyl group. However, the use of the diglycidyl ester of formula (2) is effective for forming a hygroscopic spatial network structure in the matrix due to its introduction of an alicyclic structure into the crosslinked structure.
[0119] It is desirable to use the above-mentioned crosslinking agent in an amount of 5 to 60 parts by weight, particularly 15 to 50 parts by weight, relative to 100 parts by weight of the cationic polymer. Here, it is desirable that at least 70% by weight, and preferably at least 80% by weight, of the crosslinking agent is a silane compound of the above formula (1).
[0120] Furthermore, as a crosslinking agent for introducing a crosslinked structure into anionic polymers, a compound having two or more crosslinking functional groups (e.g., epoxy groups) capable of reacting with the ionic groups present in the anionic polymer can be used. That is, diglycidyl esters represented by formula (2), which are also used in coating compositions for cationic matrices, can preferably be used:
[0121] GO(C=O)-A-(C=O)OG(2)
[0122] Wherein, G is a glycidyl group, and
[0123] A is a divalent hydrocarbon group with an aliphatic ring, such as a cycloalkylene group.
[0124] That is, in the diglycidyl ester of formula (2) above, the epoxy group reacts with the anionic group, and a cross-linked structure containing an alicyclic structure is formed in the matrix due to the divalent group A. The cross-linked structure containing the alicyclic structure is used to further suppress swelling.
[0125] In the diglycidyl esters described above, preferred examples have already been mentioned. In particular, from the viewpoint of forming a spatial network structure suitable for moisture absorption, the diglycidyl ester represented by the above formula (2-1) is most desirable.
[0126] It is desirable to use an anionic polymer crosslinking agent in an amount of 150 parts by weight, particularly 10 to 40 parts by weight, relative to 100 parts by weight of the anionic polymer.
[0127] Formation of the moisture trapping layer (B);
[0128] The aforementioned moisture-capturing layer (B) is formed by using a coating composition obtained by dispersing a hygroscopic agent in a resin serving as a matrix, and, if necessary, further dissolving or dispersing a crosslinking agent in a predetermined solvent. Specifically, the coating composition is applied to an isocyanate-based coating (C) formed on an inorganic barrier layer (A1), which will be described later, and then heated to remove the solvent. Heating and drying are typically carried out at a temperature of about 100 to about 170°C for a short time of less than 3 minutes, particularly about 0.25 to about 1 minute. This forms a moisture-capturing layer (B) that is firmly adhered to the inorganic barrier layer (A1) via the isocyanate-based coating (C).
[0129] When heated at temperatures above 100°C for an extended period (e.g., more than 1 hour), strong adhesion between the moisture-trapping layer (B) and the inorganic barrier layer (A1) can be maintained without forming an isocyanate-based coating (C) as a base layer. In this case, it is believed that the adhesion is improved due to the condensation reaction between reactive functional groups present in the matrix resin or crosslinking agent in the moisture-trapping layer (B) and silanol groups (SiOH groups) present on the surface of the inorganic barrier layer (A1).
[0130] However, as mentioned above, such a method requires prolonged heating at high temperatures, causing thermal deformation of the plastic film (A) beneath the inorganic barrier layer (A1) and self-rupture of the moisture-trapping layer (B), thus resulting in a significant reduction in production speed. Therefore, to avoid such inconvenience, the moisture-trapping layer (B) must be formed by heating at a temperature not exceeding 100°C for a short period of time.
[0131] In coating compositions used to form the moisture-trapping layer (B), there are no particular limitations if the moisture can be evaporated and removed by heating at a relatively low temperature. For example, alcoholic solvents such as methanol, ethanol, propanol, and butanol; ketone solvents such as acetone and methyl ethyl ketone; mixtures of these solvents with water; and aromatic hydrocarbon solvents such as benzene, toluene, and xylene can be used. However, when a silane compound is used as a crosslinking agent, it is desirable to use water or a mixture of water-containing solvents to promote the hydrolysis of the silane compound. Furthermore, when attempting to form a moisture-trapping layer (B) containing an anionic polymer, it is desirable to add a base (e.g., sodium hydroxide, etc.) to adjust the pH to approximately 8 to approximately 12.
[0132] The solvent described above is used in an amount that gives the coating composition a suitable viscosity for application. Furthermore, a nonionic polymer may be added in a suitable amount to adjust the viscosity of the coating composition or to adjust the water absorption rate of the formed hygroscopic matrix to be within a suitable range.
[0133] As nonionic polymers, saturated aliphatic hydrocarbon polymers such as polyvinyl alcohol, ethylene-polypropylene copolymers, and polybutene can be used; styrene polymers such as styrene-butadiene copolymers; and polyvinyl chloride can also be used. Nonionic polymers obtained by copolymerizing the above polymers with various comonomers (e.g., styrene monomers such as vinyltoluene, vinylxylene, chlorostyrene, chloromethylstyrene, α-methylstyrene, α-halostyrene, and α,β,β'-trihalostyrene; monoolefins such as ethylene and butene; and conjugated dienes such as butadiene and isoprene).
[0134] In this invention, it is desirable that the aforementioned moisture-capturing layer (B) contains, in particular, a cationic polymer as a matrix (film-forming component). That is, the moisture-capturing layer (B) containing the cationic polymer must be heated for an extended period at temperatures above 100°C to ensure exceptionally high adhesion. However, according to this invention, an isocyanate-based coating (C) is provided as a base layer. This allows for the formation of a firmly adhered moisture-capturing layer (B) without the need for prolonged heating at high temperatures, thus maximizing the advantages of this invention.
[0135] <Isocyanate-based coating (C)>
[0136] As briefly described above, in this invention, an isocyanate-based coating (C) is disposed between a plastic film (A) and a moisture-trapping layer (B). That is, the moisture-trapping layer (B) is formed on the isocyanate-based coating (C) which serves as a substrate.
[0137] Isocyanate-based coatings contain isocyanate-based polymers obtained using isocyanates as reactants as film-forming components.
[0138] In this invention, the isocyanate polymer is a polymer obtained by curing polyurethane or isocyanate reactive resin with polyisocyanate.
[0139] During the formation of the isocyanate-based coating (C), the isocyanate groups present in the coating react with MOH (where M is a metal atom such as Si) present on the surface of the inorganic barrier layer, or with ionic groups in the ionic polymer. As a result, the coating (C) exhibits high adhesion to the moisture-trapping layer (B) and effectively prevents the moisture-trapping layer (B) from delaminating.
[0140] Polyurethane;
[0141] Among the above isocyanate polymers, polyurethane is a polymer with urethane bonds (-NH-COO-) as repeating units, and is obtained through a urethane reaction of diisocyanate component and diol component.
[0142] [Diisocyanate component]
[0143] Diisocyanate components include aromatic diisocyanates, aromatic-aliphatic diisocyanates, alicyclic diisocyanates, and aliphatic diisocyanates.
[0144] Examples of aromatic diisocyanates include methyl or p-phenylene diisocyanate or mixtures thereof; 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate (NDI), 4,4'-, 2,4'- or 2,2'-diphenylmethane diisocyanate (MDI) or mixtures thereof; 2,4- or 2,6-toluene diisocyanate (TDI) or mixtures thereof; 4,4'-toluidine diisocyanate (TODI); and 4,4'-diphenyl ether diisocyanate, etc.
[0145] Examples of aromatic-aliphatic diisocyanates include 1,3- or 1,4-phenylene diisocyanate or mixtures thereof (XDI); 1,3- or 1,4-tetramethylphenylene diisocyanate or mixtures thereof (TMXDI); and ω,ω'-diisocyanate-1,4-diethylbenzene, etc.
[0146] Examples of alicyclic diisocyanates include 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanate methyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate; IPDI), 4,4'-, 2,4'- or 2,2'-dicyclohexylmethane diisocyanate or mixtures thereof (hydrogenated MDI), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,3- or 1,4-bis(isocyanate methyl)cyclohexane or mixtures thereof (hydrogenated XDI), etc.
[0147] Examples of aliphatic diisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-, 2,3- or 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, and methyl 2,6-diisocyanate hexanoate, etc.
[0148] These diisocyanate components can be used alone or in combination of two or more. Trifunctional or higher polyisocyanates may also be used in combination, depending on the requirements.
[0149] [Diol component]
[0150] The diol component includes a wide range of diols, from low molecular weight diols to oligomers. Examples include C... 2-12Alkylene glycols (e.g., ethylene glycol, 1,3- or 1,2-propanediol, 1,4-, 1,3- or 1,2-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2,2,4-trimethylpentane-1,3-diol, 1,6-hexanediol, neopentanediol, 1,5- or 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, etc.); e.g., polyoxyethylene C 2-4 Alkylene glycols include polyether glycols (e.g., diethylene glycol, triethylene glycol, tetraethylene glycol, pentylene glycol, hexaethylene glycol, heptaethylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, pentapropylene glycol, hexapropylene glycol, heptapropylene glycol, dibutyl glycol, tributyl glycol, tetrabutyl glycol, etc.); aromatic glycols (e.g., bisphenol A, diethyl terephthalate, catechol, resorcinol, hydroquinone, 1,3- or 1,4-benzenedimethanol or mixtures thereof); low molecular weight glycol components of alicyclic glycols (e.g., hydrogenated bisphenol A, hydrogenated benzyl glycol, cyclohexanediol, cyclohexanediol, etc.); polyester glycols (e.g., addition products of the above low molecular weight glycols with lactones, reaction products of the above low molecular weight glycols with dicarboxylic acids); and polycarbonate glycols (e.g., reaction products of the above low molecular weight glycols with short-chain dialkyl carbonates), etc.
[0151] The diol component can be used alone or in combination of two or more. It is also permissible to combine it with trifunctional or higher polyols as needed.
[0152] In the manufacture of polyurethane, diamine components can be further used together with diol components as needed. Diamines are used as chain extenders or crosslinking agents.
[0153] As diamines, hydrazine, for example, can be used; aliphatic diamines (e.g., ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, octamethylenediamine, etc.); aromatic diamines (e.g., meta- or p-phenylenediamine, 1,3- or 1,4-dimethylbenzenediamine or mixtures thereof, etc.); alicyclic diamines [e.g., hydrogenated xylenediamine, bis(4-aminocyclohexyl)methane, isophoronediamine, bis(4-amino-3-methylcyclohexyl)methane, etc.]. Diamines having a hydroxyl group can be further used, such as 2-hydrazinoethanol, 2-[(2-aminoethyl)amino]ethanol, etc.
[0154] The diamine component can be used alone or in combination of two or more. It is also permissible to combine it with trifunctional or higher-functional polyamine components as needed.
[0155] In this invention, the polyurethane used to form the isocyanate-based coating (C) is manufactured by dispersing or dissolving the above components in various solvents and subjecting them to widely known urethane esterification reactions.
[0156] The resulting polyurethane is preferably a high-Tg polyurethane with a glass transition point of 60°C or higher, preferably 65°C or higher, and more preferably 68°C or higher. That is, the moisture-trapping layer (B) is formed by gravure coating onto the isocyanate-based coating (C) while heating, for example, at about 60°C. The moisture-trapping layer (B) is then dried. Here, shrinkage stress during film formation or drying tends to cause cracking. However, the use of a high-Tg polyurethane is effective in preventing cracking.
[0157] The polyurethane should have a molecular weight that is substantially large enough to form a film. However, in order to form a moisture-trapping layer (B) on the isocyanate-based coating (C) and effectively prevent cracking in the coating (C), it is desirable that the weight-average molecular weight (Mw) of the polyurethane is 14,000 or more, preferably 40,000 or more, and more preferably 50,000 or more.
[0158] Furthermore, it is preferable that the isocyanate-based coating (C) formed by using polyurethane has a cross-linked structure introduced therein by at least one functional group selected from the group consisting of epoxy groups, silanol groups, and isocyanate groups. This enables the isocyanate-based coating (C) to ensure excellent adhesion to the moisture-trapping layer (B).
[0159] Cross-linking structures can be introduced by relying on functional groups. For example, a curing agent having functional groups can be added to a coating composition used to form an isocyanate-based coating (C). The cross-linking structure can then be present in the coating (C) due to curing during film formation.
[0160] Furthermore, in this invention, the polymerization / curing product obtained by reacting an isocyanate reactive resin with an isocyanate can also be used as an isocyanate-based polymer. That is, isocyanate groups are also present in the polymerization / curing product, and the coating exhibits high adhesion to the moisture-trapping layer (B) and effectively prevents the moisture-trapping layer (B) from delaminating.
[0161] Examples of isocyanate-reactive resins include those having functional groups capable of reacting with isocyanates, such as hydroxyl, carboxyl, or amino groups, particularly hydroxyl or carboxyl groups. Specifically, examples include ester resins, (meth)acrylic resins, polycarbonate resins, and polyvinyl alcohol. Furthermore, urethane resins (equivalent to the polyurethanes described above) can be used as isocyanate-reactive resins.
[0162] In particular, ester resins, (meth)acrylic resins (poly(meth)acrylic acid or poly(meth)acrylate), and urethane resins are preferably used as isocyanate reactive resins.
[0163] From the viewpoint of effectively preventing cracking during the formation of the moisture-trapping layer (B), it is desirable that the isocyanate reactive resin, like the polyurethane described above, be a high Tg resin having a glass transition point of 60°C or higher, preferably 65°C or higher, and more preferably 68°C or higher. It is also desirable that the weight-average molecular weight of the isocyanate reactive resin be 14,000 or higher, preferably 40,000 or higher, and more preferably 50,000 or higher.
[0164] Examples of isocyanates that can react with isocyanate-reactive resins include diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), isophthalene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, lysine isocyanate, isophorone diisocyanate (IPDI), and polynuclear condensates of these isocyanates, which can be used alone or in combination of two or more.
[0165] From a storage stability point of view, the ends of polyisocyanates can be capped with capping agents. Representative examples of capping agents include alcohols such as methanol, ethanol, and lactates; compounds containing phenolic hydroxyl groups such as phenol and salicylates; amides such as ε-caprolactam and 2-pyrrolidone; oximes such as acetone oxime and methyl ethyl ketone oxime; and active methylene compounds such as methyl acetoacetate, ethyl acetoacetate, acetylacetone, dimethyl malonate, and diethyl malonate, which can be used alone or in combination of two or more.
[0166] [Formation of isocyanate-based coating (C)]
[0167] An isocyanate-based coating (C) can be formed by applying a coating composition, in which a solvent in which the polyurethane or isocyanate reactive resin is dissolved or dispersed, and a curing agent having predetermined functional groups is further dispersed as needed, onto an inorganic barrier layer (A1), followed by heating and firing at a temperature above 100°C.
[0168] In this invention, from the viewpoint of forming a coating (C) in which isocyanate groups are uniformly distributed, it is desirable to use a polyurethane or isocyanate reactive resin in the form of granules for coating composition. Generally, the cumulative particle size (D50) of the resin particles, calculated from the volume measured by laser diffraction and light scattering, is in the range of 0.02 to 3 μm, particularly about 0.03 to about 1 μm.
[0169] The solvent used to form the coating composition can be a solvent that is volatile and does not require heating at a higher temperature. For example, the solvent can evaporate when heated to about 100°C. For example, water, alcohol-based organic solvents, dialkyl glycol ether-based solvents, ethylene glycol ether-based solvents, propylene glycol ether-based solvents, or mixtures thereof with water, as well as ester-based solvents, ketone-based solvents, ether-based solvents, and hydrocarbon-based solvents can be used.
[0170] The solvent is used in an amount that gives the coating composition a viscosity suitable for application.
[0171] When polyurethane resin particles are used in the coating composition, it is desirable to use a curing agent having at least one of epoxy, silanol, or isocyanate groups as functional groups, and to disperse the curing agent together with the polyurethane resin particles in a solvent. This introduces a crosslinking structure into the formed isocyanate-based coating (C), which helps to further improve adhesion to the moisture-trapping layer (B) (or the inorganic barrier layer (A1)).
[0172] As a curing agent having epoxy or silanol groups as functional groups, silane coupling agents, for example, can be used.
[0173] Examples of silane coupling agents, though not limited to these, include methyltrimethoxysilane, methyltriethoxysilane, methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrichlorosilane, vinyltriacetoxysilane, vinyltri(β-methoxyethoxy)silane, γ-methacryloyloxypropyltrimethoxysilane, γ-methacryloyloxypropyltri(β-methoxyethoxy)silane, γ-chloropropyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and hexamethyldisilazane, which can be used alone or in combination of two or more.
[0174] Among these silane coupling agents, from the viewpoint of adhesion to the moisture trapping layer (B), it is particularly desirable to use silane coupling agents containing glycidyl groups or epoxy groups, such as γ-glycidyltrimethoxysilane, γ-glycidylmethyldiethoxysilane, or β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0175] A silane coupling agent is added in an amount of 0.1 to 50 parts by weight, preferably 1 to 30 parts by weight, and more preferably 5 to 20 parts by weight, relative to 100 parts by weight of polyurethane resin particles in the coating composition.
[0176] As a curing agent having isocyanate groups as functional groups, the above-mentioned polyisocyanates can be cited as examples.
[0177] Typically, polyisocyanates are used in an amount of 1 to 50 parts by weight, preferably 5 to 40 parts by weight, and more preferably 10 to 30 parts by weight, relative to 100 parts by weight of urethane resin particles in the coating composition.
[0178] The above-mentioned silane coupling agents and polyisocyanates can be used in combination.
[0179] Furthermore, when the coating composition uses isocyanate reactive resins, particularly non-urethane resins such as ester resins or (meth)acrylic resins, the aforementioned polyisocyanates must be used as curing agents to introduce isocyanate groups.
[0180] Polyisocyanates are also used in an amount of 1 to 50 parts by weight, preferably 5 to 40 parts by weight, and more preferably 10 to 30 parts by weight, relative to 100 parts by weight of isocyanate reactive resin particles in the coating composition. The above-mentioned silane coupling agent can also be used in combination with polyisocyanates.
[0181] In this invention, various blending agents can be blended in the coating composition, as long as they do not impair the adhesion between the formed isocyanate coating (C) and the moisture-trapping layer (B).
[0182] Examples of blending agents include layered inorganic compounds, stabilizers (antioxidants, heat stabilizers, UV absorbers, etc.), plasticizers, anti-static agents, lubricants, anti-caking agents, colorants, fillers, and nucleating agents. Naturally, small amounts of resins that are not reactive to isocyanates, such as olefin resins, are permissible, as long as they do not impair adhesive properties.
[0183] <Protective Layer (D)>
[0184] In this invention, such as Figure 1 As shown, an isocyanate-based coating (C) is formed on an inorganic barrier layer (A1), and a moisture-capturing layer (B) is formed on the isocyanate-based coating (C). However, the invention is by no means limited to this embodiment. For example, as... Figure 3 As shown, it is also permissible to form a protective layer (D) on an inorganic barrier layer (A1) and to form an isocyanate coating (C) on a protective layer (D).
[0185] The protective layer (D) is designed to prevent peeling, scratching, or damage to the inorganic barrier layer (A1) after film formation. There are no particular limitations on the protective layer (D) if it does not cause the barrier film's barrier properties to deteriorate under conditions that promote testing (e.g., at 85°C-85%RH). Generally, the protective layer (D) is formed by using two or more compounds or by blending the following components (D1) and (D2).
[0186] Component (D1) is a water-soluble polymer, such as polyvinyl alcohol, polyvinylpyrrolidone, starch, methylcellulose, carboxymethylcellulose, or sodium alginate. Polyvinyl alcohol is particularly preferred.
[0187] Component (D2) is at least one compound selected from the group consisting of organoalkoxysilanes or their hydrolysis products, metal alkoxides or their hydrolysis products, and phosphorus compounds.
[0188] Organoalkoxysilanes are represented by, for example, the following formula (3):
[0189] R-Si(OR')3(3)
[0190] Where R is an organic group.
[0191] R' is an alkyl group.
[0192] Examples of organic groups include alkyl groups, as well as groups having various functional groups (e.g., (meth)acryloyl, vinyl, amino, epoxy, isocyanate, etc.).
[0193] As an alkyl group represented by R', although there are no particular limitations, examples can generally be lower alkyl groups having 4 or fewer carbon atoms (e.g., methyl, ethyl, propyl, and butyl).
[0194] Examples of organoalkoxysilanes include ethyltrimethoxysilane, (meth)acryloyloxypropyltrimethoxysilane, vinyltrimethoxysilane, glycidoxytrimethoxysilane, glycidoxypropyltrimethoxysilane, epoxycyclohexylethyltrimethoxysilane, isocyanate-propyltrimethoxysilane, and their hydrolysis products. Each can be used alone or in combination of two or more. Particularly preferred examples are glycidoxytrimethoxysilane and epoxycyclohexylethyltrimethoxysilane containing epoxy groups, and isocyanate-propyltrimethoxysilane containing isocyanate groups. Organosilanes are not limited to monomers but can also be compounds whose structure is, for example, dimer or trimer.
[0195] Metal alkoxides are compounds represented by the following formula (4):
[0196] M(OR')n(4)
[0197] Where M is a metal atom
[0198] R' is an alkyl group as in formula (3) above, and
[0199] n is an integer representing the valence of the metal atom M.
[0200] Examples of metal alkoxides include tetraethoxysilane and tripropoxyaluminum. These metal alkoxides can be used alone or in combination of two or more.
[0201] The aforementioned organoalkoxysilanes and metal alkoxides can be used as components (D2) even in the form of hydrolysis products.
[0202] Hydrolysis products can be obtained using known methods employing acids or bases. During hydrolysis, reaction catalysts such as tin compounds can be used as needed.
[0203] Examples of phosphorus compounds include phosphoric acid and its salts. Specifically, examples include orthophosphoric acid, pyrophosphoric acid, metaphosphoric acid and their alkali metal salts and ammonium salts; and trimetaphosphoric acid, tetrametaphosphoric acid, hexametaphosphoric acid, and condensed phosphoric acid such as hypermetaphosphoric acid, and their alkali metal salts and ammonium salts. Phosphoric acid esters such as triphenyl phosphate are also permitted.
[0204] These phosphorus compounds can be used alone or in combination of two or more.
[0205] The above components (D1) and (D2) are melted and mixed together at a mass ratio of (D1) / (D2) = 99 / 1 to 70 / 30. The molten mixture is then coated on the surface of the inorganic barrier layer (A1) to form a protective layer (D).
[0206] The resulting protective layer (D) has a thickness generally in the range of 0.01 to 50 μm, particularly 0.1 to 2 μm.
[0207] In the present invention Figure 1 and Figure 3 In this example, the inorganic barrier layer (A1) is formed only on one surface of the plastic film (A). However, it is also permissible to form the inorganic barrier layer (A1) on both surfaces of the film (A). Furthermore, an isocyanate-based coating (C) and a moisture-trapping layer (B) can be formed on the inorganic barrier layer (A1) formed on both surfaces.
[0208] To obtain the moisture-barrier laminate 10 of the present invention having the above-described layer structure, a moisture-capturing layer (B) is formed according to the steps described above. Thereafter, moisture is released from the moisture-capturing layer (B), and a dry film is attached to the surface of the moisture-capturing layer (B) to store the film in a protected state. When using the moisture-barrier laminate, the dry film is removed.
[0209] By further forming an isocyanate-based coating (C), the moisture-capturing layer (B) can be dry-laminated onto other barrier films, or it can be laminated onto other moisture-capturing layers (B) provided with barrier films.
[0210] <Applications>
[0211] Moisture-barrier laminates have a moisture-capturing layer that adheres tightly to the laminate without requiring prolonged high-temperature heating. From a production standpoint, this is a significant advantage.
[0212] Furthermore, it effectively prevents the moisture-trapping layer from cracking or peeling, and therefore exhibits excellent moisture barrier properties while maintaining stability. Thus, moisture-barrier laminates can be advantageously used as films for sealing various electronic devices and circuits, such as organic EL devices, solar cells, and electronic paper.
[0213] Example
[0214] <Method for measuring the glass transition temperature of isocyanate reactive resins>
[0215] A membrane made of isocyanate reactive resin was provided, and differential scanning calorimetry and quantitative analysis were performed under the following conditions. The values from the second scan were recorded.
[0216] Equipment: DSC 6220 (Differential Scanning Calorimetry) manufactured by Seiko Instrument Co.
[0217] Sample: The amount of sample, 5 to 10 mg
[0218] Measurement conditions: Nitrogen atmosphere, measured in the range of -50 to 200°C while increasing the temperature at a rate of 20°C / min.
[0219] <Methods for Measuring the Molecular Weight of Water-Dispersible Carbamate Resins>
[0220] The aqueous dispersion of the urethane polymer was freeze-dried. The resulting freeze-dried product was dissolved in dimethylformamide (MDF) eluent and adjusted. The resulting solution was allowed to stand overnight. The solution was then filtered through a 0.45 μm membrane filter. The weight-average molecular weight (Mw) of the filtrate was determined by GPC (converted to polystyrene).
[0221] Detector: Shodex RI-101
[0222] Separation column: Shodex OHpak SB-806M HQX2
[0223] Eluent: Lithium bromide in 10 mmol / L DMF
[0224] Flow rate: 1.0 ml / min
[0225] Column temperature: 50℃
[0226] <Method for determining the molecular weight of isocyanate reactive resins soluble in chloroform>
[0227] The average molecular weight of isocyanate reactive resins soluble in chloroform was measured using the following method.
[0228] Add 3 mL of solvent to approximately 10 mg of the sample, then gently stir at room temperature. After visually confirming that the sample has dissolved, filter the solvent through a 0.45 μm filter. Measure the weight-average molecular weight (Mw) of the filtrate using GPC (converted to polystyrene). Use polystyrene as a standard.
[0229] Equipment: HLC-8120 manufactured by Toso Co.
[0230] Detector: Differential refractometer RI
[0231] Columns: TSKgel Super HM-HX2 and TSKguard column Super HH as protective pillars
[0232] Medium: chloroform
[0233] Flow rate: 0.5 mL / min
[0234] Column temperature: 40℃
[0235] <Crack Assessment>
[0236] The presence of cracks was visually evaluated on A4-sized moisture barrier laminate samples. Samples with cracks occurring throughout the membrane surface were rated as ×, samples with some cracks occurring along the ends of the membrane were rated as △, and samples without cracks were rated as ○.
[0237] <Adhesion strength>
[0238] A PET film was dry-laminated onto a moisture-barrier laminate using an epoxy adhesive. To cure the adhesive layer, the laminate was aged at 50°C for 3 days. This process was used to prepare test pieces for the T-peel test.
[0239] The lamination strength (unit: N / 15mm) between the moisture barrier laminate and PET was measured using a T-type peel test at 23°C and 50%RH. The test piece was 15mm wide and 200mm long (including 50mm non-adhesive portion) at a peel speed of 300mm / min.
[0240] Test pieces with a value greater than 1N / 15mm are rated as ○, while test pieces with a value less than 1N / 15mm are rated as ×.
[0241] <Preparation of Coating Solution (B1) for Forming a Moisture-Capturing Layer Using Cationic Polymers>
[0242] A polymer solution was obtained by diluting polyallylamine (PAA-15C, aqueous solution, 15% solids, manufactured by Nittobo Medical Co.) as a cationic polymer with water to a solids content of 5% by weight.
[0243] On the other hand, a solution of the crosslinking agent is prepared by dissolving γ-glycidoxypropyltrimethoxysilane, which is used as a crosslinking agent, in water to a concentration of 5% by weight.
[0244] Next, the polymer solution and the crosslinking agent solution were mixed together such that the amount of γ-glycidoxypropyltrimethoxysilane was 20 parts by weight relative to 100 parts by weight of polyallylamine. A crosslinking product of sodium polyacrylate (TAFTIC HU-820E, aqueous dispersion, 13% solids, manufactured by Toyobo Co.) as a hygroscopic agent was further added to the mixed solution such that its amount was 420 parts by weight relative to polyallylamine. The mixture was further adjusted with water to a solids content of 5%. The mixture was thoroughly stirred to prepare a coating solution (B1) for forming a moisture-trapping layer.
[0245] <Preparation of Coating Solution (B2) for Forming a Moisture-Capturing Layer Using Anionic Polymers>
[0246] Polyacrylic acid (AC-10LP manufactured by Nihon Jyunyaku Co.), an anionic polymer, was dissolved in a mixed solvent of water / acetone (80 / 20 by weight) to achieve a solid content of 5% by weight. Sodium hydroxide was then added to neutralize the polyacrylic acid to 80%, thereby obtaining a polymer solution.
[0247] 1,2-cyclohexanedicarboxylic acid diglycidyl ester as a crosslinking agent was added to the polymer solution in an amount of 20 parts by weight relative to the partially neutralized product of polyacrylic acid. Next, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane as a binder was added in an amount of 3 parts by weight relative to the partially neutralized product of polyacrylic acid. Furthermore, a granular moisture absorbent (TAFTIC HU-820E, aqueous dispersion, 13% solids, manufactured by Toyobo Co.) was added in an amount of 431 parts by weight relative to the partially neutralized product of polyacrylic acid. The mixture was then adjusted with a water / acetone mixture (80 / 20 by weight) to achieve a total solids content of 5% by weight. The resulting mixture was then thoroughly stirred to prepare a coating solution (B2) for forming a moisture-trapping layer.
[0248] <Preparation of Coating Solution (B3) for Forming a Moisture-Capturing Layer Using a Nonionic Polymer>
[0249] A polymer solution was obtained by diluting polyvinyl alcohol (PVA 103 produced by Kuraray Co.) as a nonionic polymer with water to a solid content of 5% by weight.
[0250] On the other hand, a crosslinking agent solution was prepared by dissolving γ-glycidoxypropyltrimethoxysilane, as a crosslinking agent, in water to a concentration of 5% by weight. Next, the polymer solution and the crosslinking agent solution were mixed together such that the amount of γ-glycidoxypropyltrimethoxysilane was 20 parts by weight relative to 100 parts by weight of polyallylamine. A crosslinking product of sodium polyacrylate (TAFTIC HU-820E, aqueous dispersion, 13% solids, manufactured by Toyobo Co.), as a hygroscopic agent, was further added to the mixed solution to a concentration of 420 parts by weight relative to polyallylamine. The mixture was further adjusted with water to a solids content of 5%. The mixture was thoroughly stirred to prepare a coating solution (B3) for forming a moisture-trapping layer.
[0251] <Example 1>
[0252] A reactive isocyanate resin solution (wpb-341, 30% solids content, manufactured by Mitsui Kagaku Co.) containing water-dispersed urethane resin particles (Mw=1,000,000, glass transition point=68°C, average particle size 55nm) is provided.
[0253] An isocyanate reactive resin solution was blended with a silane coupling agent (3-epoxypropoxypropyltrimethoxysilane) as a curing agent, with the solid content of the curing agent being 5 parts by weight relative to the solid content of 100 parts by weight of the isocyanate reactive resin solution. The blend was then diluted with a mixed solvent of water and 2-propanol to prepare an isocyanate-based coating solution containing 20% solid content.
[0254] A commercially available barrier film (toppan printing, GL-RD, substrate: PET (12μm), manufactured by Toppan Insatsu Co.) with a protective layer (D) on a silicon oxide layer (inorganic barrier layer) is provided. The protective layer (D) comprises polyvinyl alcohol and tetraethoxysilane.
[0255] The above isocyanate-based coating liquid was applied to the protective layer (D) of the barrier film using a bar coater, and then heat-treated in an electric oven at a peak temperature of 100°C for 1 minute to obtain an isocyanate-based coating (C) with a thickness of 0.5 μm.
[0256] By using a bar coater, the above-mentioned water-trapping layer forming liquid (B1) containing cationic polymer is applied to the isocyanate coating (C), and heat-treated at a peak temperature of 100°C and a peak temperature holding time of 40 seconds to form a 4 μm thick water-trapping layer (B), thereby obtaining a water-barrier laminate 10.
[0257] <Example 2>
[0258] Except that the amount of curing agent solid component relative to 100 parts by weight of the main polymer solution was changed to 20 parts by weight, the isocyanate-based coating solution was prepared in the same manner as in Example 1.
[0259] In addition to using the above isocyanate-based coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 1.
[0260] <Example 3>
[0261] The isocyanate reactive resin solution provided in Example 1 was used. This solution was blended with a terminal isocyanate (XWB-F206MEDG manufactured by Mitsui Kagaku Co.) as a curing agent at a curing agent content of 10 parts by weight relative to 100 parts by weight of the solid component of the main agent. The blend was diluted with a mixed solvent of water and 2-propanol to prepare an isocyanate-based coating solution containing 20% solid component.
[0262] In addition to using the above isocyanate-based coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 1.
[0263] <Example 4>
[0264] Except that the amount of curing agent solid component relative to 100 parts by weight of the isocyanate reactive resin solution was changed to 30 parts by weight, the isocyanate-based coating liquid was prepared in the same manner as in Example 3.
[0265] In addition to using the above isocyanate-based coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 1.
[0266] <Example 5>
[0267] Except that the amount of curing agent solid component relative to 100 parts by weight of the isocyanate reactive resin solution was changed to 50 parts by weight, the isocyanate-based coating liquid was prepared in the same manner as in Example 3.
[0268] In addition to using the above isocyanate-based coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 1.
[0269] <Example 6>
[0270] An isocyanate-based coating (C) is formed on the protective layer (D) of a commercially available barrier film with a thickness of 0.5 μm in the same manner as in Example 3.
[0271] A water-trapping layer forming liquid (B2) containing an anionic polymer is applied to the above isocyanate-based coating (C) using a bar coater, and then heat-treated at a peak temperature of 100°C and a peak temperature holding time of 40 seconds to obtain a water-barrier laminate 10.
[0272] <Example 7>
[0273] Except for forming a 4 μm thick moisture-trapping layer (B) by using a coating liquid (B3) containing a nonionic polymer as a coating material for forming the moisture-trapping layer, the moisture-barrier laminate 10 was obtained in the same manner as in Example 6.
[0274] <Example 8>
[0275] A commercially available barrier film (Techbarrier LX, substrate: PET 12μm, manufactured by Mitsubishi Jushi Co.) is provided, which has a silicon oxide layer as an inorganic barrier layer but no protective layer (D).
[0276] Isocyanate-based coating solutions were prepared in the same manner as in Example 3.
[0277] An isocyanate-based coating liquid was applied to the inorganic barrier layer of the above barrier film using a bar coater, and then heat-treated in an electric oven at a peak temperature of 100°C for 1 minute to form a 0.5 μm thick isocyanate-based coating (C).
[0278] A water-trapping layer (B1) containing a cationic polymer is applied to the above isocyanate-based coating (C) using a bar coater, and then heat-treated at a peak temperature of 100°C and a peak temperature holding time of 40 seconds to form a 4 μm thick water-trapping layer (B1), thereby obtaining a water-barrier laminate 10.
[0279] <Example 9>
[0280] The isocyanate-based coating solution was prepared in the same manner as in Example 3. Using the isocyanate-based solution, a urethane coating (C) was formed on the protective layer (D) of a commercially available barrier film in the same manner as in Example 1, and a moisture-trapping layer (B) containing a cationic polymer was further formed thereon.
[0281] Next, using a bar coater, the above-mentioned urethane coating solution is applied to the other surface of the barrier film (the surface of the PET film) on which the isocyanate-based coating (C) and moisture-trapping layer (B) have been formed as described above. Then, the urethane coating solution is heat-treated in an electric oven at a peak temperature of 100°C for 3 minutes to form an isocyanate-based coating (C) with a thickness of 0.5 μm.
[0282] Furthermore, using a bar coater, a water-trapping layer forming liquid (B1) containing a cationic polymer is applied to an isocyanate-based coating (C) already formed on another surface. The water-trapping layer forming liquid (B1) is then heat-treated at a peak temperature of 100°C and a peak temperature holding time of 40 seconds to form a water-trapping layer (B) with a thickness of 4 μm. This yields a moisture-barrier laminate 10 having a water-trapping layer (B) on both surfaces.
[0283] <Example 10>
[0284] A main polymer solution (Aracoat DA-105, 30% solids, produced by Arakawa Kagaku Kogyo C.) containing an acrylic resin (Mw=69,000, glass transition point=70°C) is provided.
[0285] The main polymer solution was blended with a polyisocyanate (D-110N manufactured by Mitsui Kagaku Co.) as a curing agent at a solid content of 10 parts by weight relative to 100 parts by weight of the main polymer solution. The blend was then diluted with methyl ethyl ketone to prepare an isocyanate-based coating solution containing 20% solid content.
[0286] A commercially available barrier film (Toppan Printing, GX, Substrate: PET (12μm), manufactured by Toppan Insatsu Co.) with a protective layer (D) on an alumina layer (inorganic barrier layer) is provided. The protective layer (D) comprises polyvinyl alcohol and tetraethoxysilane.
[0287] The above isocyanate-based coating solution was applied to the protective layer (D) of the barrier film using a bar coater, and then heat-treated in an electric oven at a peak temperature of 100°C for 1 minute to obtain an isocyanate-based coating (C) with a thickness of 0.5 μm.
[0288] A water-trapping layer forming liquid (B1) containing a cationic polymer was applied to an isocyanate-based coating (C) using a bar coater. The water-trapping layer forming liquid (B1) was then heat-treated at a peak temperature of 100°C and a peak temperature holding time of 40 seconds to form a 4 μm thick water-trapping layer (B), thereby obtaining a water-barrier laminate 10.
[0289] <Example 11>
[0290] Except that the amount of curing agent solid component relative to 100 parts by weight of the main polymerization solution was changed to 20 parts by weight, the isocyanate-based coating liquid was prepared in the same manner as in Example 10.
[0291] In addition to using the above isocyanate-based coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 10.
[0292] <Example 12>
[0293] Polyester resin (Vylon GK880, Mw=55,000, glass transition point=81℃, manufactured by Toyobo Co.) was diluted with methyl ethyl ketone (MEK) to prepare an anchor coating solution containing 20% solids.
[0294] The main polymer solution was blended with a polyisocyanate (D-110N manufactured by Mitsui Kagaku Co.) as a curing agent at a solid content of 10 parts by weight relative to 100 parts by weight of the main polymer solution. The blend was then diluted with methyl ethyl ketone to prepare a urethane coating solution containing 20% solid content.
[0295] In addition to using the above isocyanate-based coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 10.
[0296] <Example 13>
[0297] A master polymer solution containing polyester resin (Mw=14,000, glass transition point=83°C) is provided (Elitel KA-3356 manufactured by Unitika Co.).
[0298] The main polymer solution was blended with a terminal isocyanate (XWB-F206 MEDG manufactured by Mitsui Kagaku Co.) as a curing agent at a ratio of 10 parts by weight of the solid content of the curing agent to 10 parts by weight of the solid content of the main polymer solution for every 100 parts by weight. The blend was then diluted with a mixed solvent of water and 2-propanol to prepare an isocyanate-based coating solution containing 20% solid content.
[0299] A commercially available barrier film (Toppan Printing, GX, Substrate: PET (12μm), manufactured by Toppan Insatsu Co.) with a protective layer (D) on an alumina layer (inorganic barrier layer) is provided. The protective layer (D) comprises polyvinyl alcohol and tetraethoxysilane.
[0300] The above isocyanate-based coating liquid was applied to the protective layer (D) of the barrier film using a bar coater, and then heat-treated in an electric oven at a peak temperature of 130°C for 5 minutes to obtain an isocyanate-based coating (C) with a thickness of 0.5 μm.
[0301] A water-trapping layer forming liquid (B1) containing a cationic polymer was applied to an isocyanate-based coating (C) using a bar coater. The water-trapping layer forming liquid (B1) was then heat-treated at a peak temperature of 100°C and a peak temperature holding time of 40 seconds to form a 4 μm thick water-trapping layer (B), thereby obtaining a water-barrier laminate 10.
[0302] <Example 14>
[0303] A master polymer solution containing polyester resin (Mw=41,000, glass transition point=68°C) (Elitel KT-8803 manufactured by Unitika Co.) is provided.
[0304] The main polymer solution was blended with isocyanate (WD-725 manufactured by Mitsui Kagaku Co.) as a curing agent at a ratio of 10 parts by weight of curing agent solids to 100 parts by weight of main polymer solution solids. The blend was then diluted with a mixed solvent of water and 2-propanol to prepare an isocyanate-based coating solution containing 20% solids.
[0305] In addition to using the above isocyanate-based coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 10.
[0306] <Example 15>
[0307] Polyester resin (Vylon V600, Mw=39,000, glass transition point=47°C, manufactured by Toyobo Co.) was diluted with methyl ethyl ketone (MEK) to prepare an anchoring coating solution containing 20% solids.
[0308] The main polymer solution provided in Comparative Example 1 was used. The main polymer solution was blended with a polyisocyanate (D-110N manufactured by Mitsui Kagaku Co.) as a curing agent at a ratio of 10 parts by weight of the solid content of the curing agent to 10 parts by weight of the solid content of the main agent for every 100 parts by weight. The blend was then diluted with methyl ethyl ketone to prepare a urethane coating solution containing 20% solid content.
[0309] In addition to using the above-mentioned urethane coating liquid, a moisture-barrier laminate 10 was obtained by the same method as in Example 10.
[0310] <Comparative Example 1>
[0311] Polyester resin (Vylon V600, Mw=39,000, manufactured by Toyobo Co.) was diluted with methyl ethyl ketone (MEK) to prepare an anchoring coating solution containing 20% solids.
[0312] Except for forming a layer below the moisture-trapping layer (B) by changing the anchoring coating liquid in the isocyanate-based coating liquid, the moisture-barrier laminate 10 is obtained by the same method as in Example 10.
[0313] <Comparative Example 2>
[0314] Except for forming a 4 μm thick moisture-trapping layer (B) by coating a moisture-trapping layer forming liquid (B1) containing a cationic polymer onto the protective layer (D) of the barrier film, without forming an isocyanate-based coating (C), the moisture-blocking laminate 10 is obtained in the same manner as in Example 1.
[0315] <Comparative Example 3>
[0316] A commercially available barrier film is provided, which has a silicon oxide layer, also used in Example 10, as an inorganic barrier layer, but without a protective layer (D).
[0317] A water-barrier laminate 10 was obtained by forming a 4 μm thick water-capturing layer (B) containing a cationic polymer on the inorganic barrier layer of the barrier film, as in Comparative Example 2.
[0318] <Evaluation Experiment>
[0319] The various properties of the moisture-barrier laminate 10 prepared above were measured using the methods described above. The results are shown in Table 1.
[0320] [Table 1]
[0321]
[0322] mark This indicates that no protective layer D was formed.
[0323] Explanation of reference numerals in the attached figures
[0324] (A): Plastic film
[0325] (A1): Inorganic barrier layer
[0326] (B): Moisture trapping layer
[0327] (C): Isocyanate-based coatings
[0328] (D): Protective layer
[0329] 10: Moisture-barrier laminate.
Claims
1. A moisture-barrier laminate comprising a plastic film (A) having an inorganic barrier layer (A1) on its surface and a moisture-capturing layer (B), characterized in that, Between the inorganic barrier layer (A1) and the moisture trapping layer (B), an isocyanate-based coating (C) is provided, which contains an isocyanate-based polymer obtained by reacting isocyanate as a reactive component as a film-forming component. and The moisture-capturing layer (B) is formed on the isocyanate-based coating (C) which serves as a substrate. The isocyanate polymer is a high-Tg urethane resin with a glass transition point above 60°C, in which a cross-linking structure is introduced by at least one functional group selected from the group consisting of epoxy groups, silanol groups, and isocyanate groups. The high Tg urethane resin has a weight-average molecular weight (Mw) of 50,000 or higher.
2. A moisture-barrier laminate comprising a plastic film (A) having an inorganic barrier layer (A1) on its surface and a moisture-capturing layer (B), characterized in that, Between the inorganic barrier layer (A1) and the moisture trapping layer (B), an isocyanate-based coating (C) is provided, which contains an isocyanate-based polymer obtained by reacting isocyanate as a reactive component as a film-forming component. and The moisture-capturing layer (B) is formed on the isocyanate-based coating (C) which serves as a substrate. The isocyanate-based polymer is formed by curing isocyanate reactive resin using polyisocyanate as a curing agent. The isocyanate reactive resin is a (meth)acrylic resin and has a glass transition point above 60°C. The weight-average molecular weight (Mw) of the isocyanate reactive resin is 50,000 or higher.
3. The moisture-barrier laminate according to claim 1 or 2, wherein the moisture-capturing layer (B) contains a hygroscopic polymer.
4. The moisture-barrier laminate according to claim 3, wherein the moisture-capturing layer (B) has a structure in which a desiccant with a lower reach of humidity than the matrix is dispersed in a hygroscopic matrix of an ionic polymer.
5. The moisture-barrier laminate according to claim 4, wherein the ionic polymer contained in the moisture-capturing layer (B) is a cationic polymer.
6. The moisture-barrier laminate according to claim 1 or 2, wherein a protective layer (D) is provided between the inorganic barrier layer (A1) and the isocyanate coating (C).
7. The moisture-barrier laminate according to claim 6, wherein the protective layer (D) contains a water-soluble polymer component (D1) and at least one component (D2) selected from the group consisting of organoalkoxysilanes or their hydrolysis products, metal alkoxides or their hydrolysis products, and phosphorus compounds.
8. A sealing material for electronic devices, comprising the moisture-barrier laminate according to any one of claims 1-7.
9. A coating composition for forming a base layer of a moisture trapping layer, the coating composition being obtained by dissolving or dispersing urethane-based resin particles having a glass transition point of 60°C or higher in a solvent, characterized in that, The solvent contains a curing agent dissolved or dispersed therein, having at least one functional group selected from the group consisting of epoxy groups, silanol groups, and isocyanate groups. The urethane resin particles are formed from urethane polymers with a weight-average molecular weight (Mw) of 50,000 or more.
10. The coating composition according to claim 9, wherein the urethane resin particles have a particle size of 0.02 to 3 μm.
11. The coating composition according to claim 9, wherein, As the curing agent, the polyisocyanate is contained in an amount of 1 to 50 parts by weight relative to 100 parts by weight of the urethane resin particles.
12. The coating composition according to claim 9, wherein, As the curing agent, the silane coupling agent is contained in an amount of 0.1 to 50 parts by weight relative to 100 parts by weight of the urethane resin particles.
13. A coating composition for forming a base layer of a moisture capturing layer, the coating composition for forming a base layer of a moisture capturing layer comprising a coating composition obtained by dissolving or dispersing isocyanate-reactive resin particles in a solvent, characterized in that, The solvent contains a polyisocyanate dissolved or dispersed therein as a curing agent. The isocyanate reactive resin is a (meth)acrylic resin and has a glass transition point above 60°C. The weight-average molecular weight (Mw) of the isocyanate reactive resin is 50,000 or higher.
Citation Information
Patent Citations
Plastic container and manufacture thereof