A bimetallic lead-silver catalyst and a preparation method and application thereof

Bimetallic lead-silver catalysts were prepared by in-situ electrodeposition-displacement method, which solved the problem of difficult generation of active species in Pb-based catalysts and enabled the efficient electrohydrogenation reaction of levulinic acid. The catalysts exhibited excellent 4-hydroxyvalerate synthesis performance at low potentials.

CN122358247APending Publication Date: 2026-07-10FUDAN UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610660429.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-14
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

The formation of active species in existing Pb-based electrocatalysts is difficult, resulting in poor performance of the electrohydrogenation reaction of levulinic acid, especially with low space-time yield and Faraday efficiency at high potentials.

Method used

Bimetallic lead-silver catalysts were prepared by in-situ electrodeposition-displacement method. By loading lead and silver stepwise on a carbon paper substrate to form a sheet-like structure, the synergistic effect of active sites was achieved, avoiding the side reaction of hydrogen evolution at the cathode.

Benefits of technology

High space-time yield and high faradaic efficiency were achieved at a lower reaction potential, significantly improving catalyst performance. The space-time yield of 4-hydroxyvalerate reached 1.39 mmol·h-1·cm-2, the selectivity was close to 100%, and the faradaic efficiency reached 93.5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122358247A_ABST
    Figure CN122358247A_ABST
Patent Text Reader

Abstract

This invention relates to a hydrogenation catalyst for levulinic acid, specifically a bimetallic lead-silver catalyst, its preparation method, and its application. The preparation method includes the following steps: S1: ultrasonic treatment of a substrate in distilled water; S2: using the substrate treated in step S1 as a working electrode, performing cathodic electrodeposition in an acidic electrolyte containing lead salt to obtain E-Pb@C; S3: placing the E-Pb@C obtained in step S2 in a solution containing silver salt to perform an in-situ exchange reaction to obtain the E-PbAg@C catalyst. Compared with the prior art, this invention solves the problem of poor performance caused by the difficulty in generating active species on Pb-based electrocatalysts in the prior art. The bimetallic lead-silver catalyst of this scheme is used for the electrocatalytic hydrogenation of levulinic acid, achieving both high space-time yield and high Faradaic efficiency at a relatively low reaction potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a hydrogenation catalyst for levulinic acid, specifically to a bimetallic lead-silver catalyst and its preparation method and application. Background Technology

[0002] The non-renewable nature of fossil fuels has made the development of sustainable energy and resource utilization technologies a major research focus. Biomass, as the only widely available renewable organic carbon source, has yielded a series of platform compounds with enormous development potential. Levulpropionic acid, an important chemical in this field, can be obtained through multi-step conversion of carbohydrates. Further hydrogenation of its ketone carbon group can synthesize high-value-added 4-hydroxyvalerate, which can be widely used in polymer and pharmaceutical synthesis industries. However, current traditional thermocatalytic hydrogenation relies heavily on high-temperature, high-pressure hydrogen reaction conditions, resulting in high energy consumption and significant safety risks. In contrast, electrocatalytic hydrogenation offers a milder, water-based, green synthesis technology, thus attracting considerable attention in recent years.

[0003] Existing electrohydrogenation catalysts for levulinic acid are mainly Pb-based electrodes. For example, Schröder et al. used Pb sheets at -1.80 V. RHE At the operating potential, ~19% substrate conversion, ~48% γ-valerol selectivity, and ~21% Faraday efficiency were achieved (RSC Adv., 2015, 5, 26634-26643); Lucas et al. used a Pb electrode at 50°C and -1.90V. RHE Under the desired reaction conditions, a substrate conversion of 84.6%, a 4-hydroxyvalerate selectivity of >99.9%, and a Faraday efficiency of 84.6% were further achieved (Green Chem., 2021, 23, 9154-9164). Han et al., by controlling the chemical state of Pb species, used partially oxidized PbS with an ionic liquid electrolyte at -2.15 V. Ag / AgCl A Faraday efficiency of 78.6% was achieved (Chem. Sci., 2019, 10, 1754-1759); Chinese patent CN116536691A discloses a catalyst based on Fe2O3 / PbO2 precursor, which achieves a Faraday efficiency of 78.6% at -1.10 V. RHE It achieves nearly 100% selectivity for γ-valerol and 59.2% Faraday efficiency.

[0004] Therefore, current technologies still suffer from performance deficiencies due to the difficulty in generating active species in Pb-based electrocatalysts. There is an urgent need to develop a simple in-situ preparation method to synthesize an electrohydrogenation catalyst for levulinic acid with excellent activity, thereby reducing the reaction potential on Pb-based catalysts and achieving high space-time yield and Faraday efficiency of 4-hydroxyvalerate. Summary of the Invention

[0005] The purpose of this invention is to provide a bimetallic lead-silver catalyst, its preparation method, and its application to solve at least one of the aforementioned problems, thereby addressing the issue of poor performance caused by the difficulty in generating active species on Pb-based electrocatalysts in the prior art. The bimetallic lead-silver catalyst of this invention is used for the electrocatalytic hydrogenation of levulinic acid, achieving both high space-time yield and high Faradaic efficiency at a relatively low reaction potential.

[0006] The objective of this invention is achieved through the following technical solution: The first aspect of this invention discloses a method for preparing a bimetallic lead-silver catalyst, comprising the following steps: S1: Place the substrate in distilled water for ultrasonic treatment; S2: Using the substrate treated in step S1 as the working electrode, it is subjected to cathodic electrodeposition in an acidic electrolyte containing lead salt to obtain E-Pb@C; S3: The E-Pb@C obtained in step S2 is placed in a solution containing silver salt to carry out an in-situ substitution reaction to obtain the E-PbAg@C catalyst.

[0007] Preferably, in step S1, The substrate is carbon paper; Before being subjected to ultrasonic treatment in distilled water, the substrate is first subjected to ultrasonic treatment in anhydrous ethanol.

[0008] Preferably, in step S2, The lead salt is selected from one of lead acetate, lead nitrate, lead fluoroborate, and lead perchlorate; The concentration of the lead salt in the acidic electrolyte is 5 to 100 mmol / L.

[0009] Preferably, in step S2, The solute in the acidic electrolyte is one of acetic acid, nitric acid, fluoroboric acid, and perchloric acid; The pH value of the acidic electrolyte is 1 to 4.

[0010] Preferably, in step S2, The conditions for the cathode electrodeposition are as follows: The temperature is 25℃, and the potential is -0.10~-0.60 V. RHE The time is 5 to 30 minutes; The product obtained by cathodic electrodeposition was washed with deionized water until neutral and then dried overnight under vacuum to obtain E-Pb@C.

[0011] Preferably, in step S3, The silver salt is selected from one of silver nitrate, silver fluoroborate, and silver perchlorate; The concentration of the silver salt is 1-50 mmol / L; The molar ratio of silver salt to lead salt is 0 to 4:1, and is not 0.

[0012] Preferably, in step S3, The conditions for the in-situ exchange reaction are as follows: The temperature is 25℃, and the time is 2~30 minutes; The product obtained from the in-situ substitution reaction was washed with deionized water until neutral and then dried under vacuum overnight to obtain the E-PbAg@C catalyst.

[0013] The second aspect of this invention discloses a bimetallic lead-silver catalyst, which is prepared by any of the preparation methods described above; The active metal component of the bimetallic lead-silver catalyst has a plate-like morphology.

[0014] The third aspect of this invention discloses the application of a bimetallic lead-silver catalyst as described above in the electrocatalytic hydrogenation of levulinic acid to synthesize 4-hydroxyvalerate.

[0015] Preferably, the reaction conditions for the electrocatalytic hydrogenation are as follows: The temperature is 25℃ and the potential is -1.38 V. RHE .

[0016] The working principle of this invention is as follows: This scheme employs an in-situ electrodeposition-displacement method to achieve stepwise loading of metal components. The resulting lead-silver catalyst alters the electronic state structure of the active sites through bimetallic synergy, thereby regulating the generation energy of electrohydrogenation active species during the reaction. This allows the reaction to proceed at a relatively low potential, promoting hydrogenation activity while avoiding side reactions, thus achieving both high space-time yield and high Faradaic efficiency.

[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention proposes an in-situ preparation method for a bimetallic lead-silver catalyst. The method is simple, rapid, and mild. It achieves stepwise loading of electrohydrogenation active sites through in-situ electrodeposition-displacement, and can be used directly as a pre-assembled electrode. On the one hand, it avoids the complex and relatively harsh hydrothermal or thermal reduction process and the addition of binders in the traditional electrode preparation process. On the other hand, it realizes the rational introduction and control of the second metal component.

[0018] The resulting bimetallic catalyst has a plate-like structure, providing open catalytic active sites compared to commercially available metal electrodes. The synergistic effect of the bimetallic lead-silver combination promotes the generation of active species during the reaction process while avoiding the occurrence of the cathode hydrogen evolution side reaction. This achieves a simultaneous increase in the space-time yield and Faraday efficiency of 4-hydroxyvalerate at a relatively mild potential, and has application potential in large-scale electrocatalytic hydrogenation of biomass-derived compounds and related fields.

[0019] This invention achieves simple and rapid construction of binder-free electrocatalysts through in-situ electrodeposition-displacement method, optimizes the active area of ​​metal sites, and utilizes the synergistic effect of bimetallic lead-silver to achieve the desired effect at -1.38 V. RHE Achieving 1.39 mmol·h -1 ·cm -2 The invention achieves a high space-time yield, nearly 100% product selectivity, and 93.5% Faradaic efficiency for 4-hydroxyvalerate. Compared with existing technologies, this invention solves the problems of excessively high hydrogenation reaction potential, low space-time yield, and low Faradaic efficiency caused by the difficulty in generating active species in Pb-based catalysts. Attached Figure Description

[0020] Figure 1 The image shows the XRD pattern of the product from Example 1.

[0021] Figure 2 The image shows the XPS spectrum of the product from Example 1.

[0022] Figure 3 Linear sweep voltammetry (LSV) curves were obtained with or without levulinic acid in 0.5M PBS (pH=7.5) electrolyte when the product of Example 1 was used as the working electrode. Detailed Implementation

[0023] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.

[0024] Unless otherwise specified in the following description, the reagents used are conventional commercial products, the methods used are well-known in the art, and any other matters not covered herein may be handled using existing technologies.

[0025] An in-situ preparation method for a bimetallic lead-silver catalyst, wherein the catalyst is obtained by in-situ electrodeposition-displacement method, specifically including the following steps: S1: The carbon paper substrate is ultrasonically treated in anhydrous ethanol to clean the surface, and then ultrasonically treated in distilled water to ensure its hydrophilicity. S2: Using the carbon paper substrate obtained in step S1 as the working electrode, cathodic electrodeposition is performed in an acidic electrolyte containing divalent lead salt. The electrodeposition product is washed and vacuum dried to obtain E-Pb@C. S3: The E-Pb@C obtained in step S2 was placed in a solution containing monovalent silver salt to carry out an in-situ substitution reaction. The substitution reaction product was washed and dried to obtain the E-PbAg@C catalyst.

[0026] Preferably, the divalent lead salt is selected from one of lead acetate, lead nitrate, lead fluoroborate, and lead perchlorate, and the monovalent silver salt is selected from one of silver nitrate, silver fluoroborate, and silver perchlorate.

[0027] Preferably, the concentration of the divalent lead salt is 5-100 mmol / L; the concentration of the monovalent silver salt is 1-50 mmol / L. The molar ratio of silver salt to lead salt is 0 to 4:1, and is not 0.

[0028] Preferably, the pH value of the acidic electrolyte is 1 to 4; the solute of the acidic electrolyte is one of acetic acid, nitric acid, fluoroboric acid, and perchloric acid.

[0029] Preferably, the cathode electrodeposition temperature is 25°C and the potential is -0.10 to -0.60 V. RHE The washing time is 5-30 min; the obtained product is washed with deionized water until neutral and then dried under vacuum overnight.

[0030] Preferably, the in-situ substitution reaction temperature is 25°C and the time is 2-30 min; the obtained product is washed with deionized water until neutral and then dried under vacuum overnight.

[0031] A second aspect of this invention discloses a bimetallic lead-silver catalyst prepared by the method described above. This E-PbAg@C electrohydrogenation catalyst uses carbon fiber as a substrate, with the metal active component exhibiting a plate-like morphology, and silver species supported on the surface of lead species, forming a bimetallic interface.

[0032] The third aspect of this invention discloses the application of the bimetallic lead-silver catalyst described above in the electrocatalytic hydrogenation of levulinic acid. The reaction conditions for this E-PbAg@C catalyst are: reaction temperature 25°C, reaction potential -1.38 V. RHE .

[0033] Example 1 Add 1.32 g of Pb(NO3)2 to 40 mL of distilled water until completely dissolved, then gradually add 1 M nitric acid solution until the pH of the solution reaches 2, thus creating the precursor solution. After stirring at room temperature for 40 min, immerse pre-ultrasonic-cleaned carbon paper (anhydrous ethanol + distilled water) into the precursor solution, and incubate at -0.20 V. RHE Deposition for 30 min. After deposition, wash with deionized water until neutral, then dry under vacuum overnight.

[0034] The synthesized material was immersed in a solution containing 20 mM AgNO3 and reacted at room temperature for 20 min. After washing with deionized water until neutral, it was dried under vacuum overnight. The resulting material was denoted as E-PbAg@C.

[0035] Figure 1 The XRD pattern showed that the catalyst prepared in Example 1 exhibited diffraction signals of Pb and PbO. The oxidized species may have originated from the surface oxidation process of metallic lead in air. No diffraction signal of Ag was observed, indicating that the Ag species had a low content or high dispersion. Figure 2 The XPS spectra show that the Pb species in the catalyst exist in both 0 and +2 valence states, while the Ag species remain in 0 valence. Figure 3 The LSV curves show that when levulinic acid is added, E-PbAg@C exhibits a larger reaction current compared to when no substrate is added. This indicates that the kinetics of levulinic acid electrohydrogenation on E-PbAg@C are significantly better than the cathode hydrogen evolution side reaction, verifying its excellent performance.

[0036] Example 2 The catalyst synthesis process was basically the same as in Example 1, except that the mass of Pb(NO3)2 was changed to 0.265g, and other conditions were the same as in Example 1. The resulting catalyst was denoted as E-PbAg@C-2.

[0037] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0038] Example 3 The catalyst synthesis process was basically the same as in Example 1, except that the mass of Pb(NO3)2 was changed to 0.066g, and other conditions were the same as in Example 1. The resulting catalyst was denoted as E-PbAg@C-3.

[0039] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0040] Example 4 The catalyst synthesis process is basically the same as in Example 1, except that the deposition potential is changed to -0.40 V. RHEOther conditions were the same as in Example 1, and the resulting catalyst was denoted as E-PbAg@C-4.

[0041] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0042] Example 5 The catalyst synthesis process is basically the same as in Example 1, except that the deposition potential is changed to -0.60 V. RHE Other conditions were the same as in Example 1, and the resulting catalyst was denoted as E-PbAg@C-5.

[0043] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0044] Example 6 The catalyst synthesis process was basically the same as in Example 1, except that the deposition time was changed to 5 min and other conditions were the same as in Example 1. The resulting catalyst was denoted as E-PbAg@C-6.

[0045] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0046] Example 7 The catalyst synthesis process was basically the same as in Example 1, except that the deposition time was changed to 10 min and other conditions were the same as in Example 1. The resulting catalyst was denoted as E-PbAg@C-7.

[0047] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0048] Example 8 The catalyst synthesis process was basically the same as in Example 1, except that the concentration of AgNO3 was changed to 2mM, and other conditions were the same as in Example 1. The resulting catalyst was denoted as E-PbAg@C-8.

[0049] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0050] Example 9 The catalyst synthesis process was basically the same as in Example 1, except that the concentration of AgNO3 was changed to 50 mM, and other conditions were the same as in Example 1. The resulting catalyst was denoted as E-PbAg@C-9.

[0051] After testing, its performance is basically the same as that of Example 1, and will not be described in detail here.

[0052] Comparative Example 1 An aqueous solution of 100 mM Pb(NO3)2 (pH=2) was used as the precursor solution. Pre-ultrasonically cleaned carbon paper was immersed in the precursor solution at -0.20 V. RHEDeposition was carried out for 30 min. After deposition, the catalyst was washed with deionized water until neutral and then dried under vacuum overnight. The resulting catalyst was denoted as E-Pb@C.

[0053] Comparative Example 2 Add 0.068 g AgNO3 to 40 ml of distilled water until completely dissolved to prepare the precursor solution. After stirring at room temperature for 40 min, immerse pre-ultrasonic-cleaned carbon paper in the precursor solution and incubate at -0.30 V. RHE Deposition was carried out for 30 min. After deposition, the catalyst was washed with deionized water until neutral and then dried under vacuum overnight. The resulting catalyst was designated E-Ag@C.

[0054] Comparative Example 3 An aqueous solution (pH=2) containing 100 mM Pb(NO3)2 and 10 mM AgNO3 was used as the precursor solution. Pre-ultrasonically cleaned carbon paper was immersed in the precursor solution at -0.20 V. RHE Deposition was carried out for 30 min. After deposition, the catalyst was washed with deionized water until neutral and then dried under vacuum overnight. The resulting catalyst was designated as E-PbAg@C-10.

[0055] Performance testing: The performance of catalysts E-PbAg@C (Example 1), E-Pb@C (Comparative Example 1), E-Ag@C (Comparative Example 2), and E-PbAg@C-10 (Comparative Example 3) in the electrohydrogenation of 4-hydroxyvalerate from levulinic acid was compared. The performance of the catalysts was evaluated using a 0.5M PBS solution (pH=7.5) containing 0.9M levulinic acid as the electrolyte. The electrohydrogenation reaction of levulinic acid was carried out in a 10mL H-type electrolytic cell at a reaction temperature of 25°C and a reaction potential of -1.38 V. RHE The reaction time was 3 hours. After the electrohydrogenation reaction was completed, the substrate and product in the electrolyte were quantitatively analyzed by high-performance liquid chromatography (HPLC), and the reaction performance parameters were calculated. The reaction performance of each electrocatalyst is shown in Table 1.

[0056] Table 1 Summary of performance test results for Example 1 and Comparative Examples 1-3 According to the results in Table 1, the E-PbAg@C catalyst prepared in situ using the present invention exhibits excellent space-time yield, selectivity and Faraday efficiency of 4-hydroxyvalerate in the electrohydrogenation reaction of levulinic acid, which is significantly better than the single-metal components E-Pb@C, E-Ag@C and E-PbAg@C-10 with bimetallic components simultaneously loaded in situ.

[0057] In summary, this invention achieves simple and rapid construction of an electrocatalyst without binders through an in-situ electrodeposition-displacement method, optimizes the active area of ​​the metal sites, and utilizes the synergistic effect of the bimetallic lead-silver combination at -1.38 V. RHE The concentration of 1.39 mmol·h was achieved. -1 ·cm -2 The invention achieves a high space-time yield, nearly 100% product selectivity, and 93.5% Faradaic efficiency for 4-hydroxyvalerate. Compared with existing technologies, this invention solves the problems of excessively high hydrogenation reaction potential, low space-time yield, and low Faradaic efficiency caused by the difficulty in generating active species in Pb-based catalysts.

[0058] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a bimetallic lead-silver catalyst, characterized in that, Includes the following steps: S1: Place the substrate in distilled water for ultrasonic treatment; S2: Using the substrate treated in step S1 as the working electrode, it is subjected to cathodic electrodeposition in an acidic electrolyte containing lead salt to obtain E-Pb@C; S3: The E-Pb@C obtained in step S2 is placed in a solution containing silver salt to carry out an in-situ substitution reaction to obtain the E-PbAg@C catalyst.

2. The method for preparing a bimetallic lead-silver catalyst according to claim 1, characterized in that, In step S1, The substrate is carbon paper; Before being subjected to ultrasonic treatment in distilled water, the substrate is first subjected to ultrasonic treatment in anhydrous ethanol.

3. The method for preparing a bimetallic lead-silver catalyst according to claim 1, characterized in that, In step S2, The lead salt is selected from one of lead acetate, lead nitrate, lead fluoroborate, and lead perchlorate; The concentration of the lead salt in the acidic electrolyte is 5 to 100 mmol / L.

4. The method for preparing a bimetallic lead-silver catalyst according to claim 1, characterized in that, In step S2, The solute in the acidic electrolyte is one of acetic acid, nitric acid, fluoroboric acid, and perchloric acid; The pH value of the acidic electrolyte is 1 to 4.

5. The method for preparing a bimetallic lead-silver catalyst according to claim 1, characterized in that, In step S2, The conditions for the cathode electrodeposition are as follows: The temperature is 25℃, and the potential is -0.10~-0.60 V. RHE The time is 5 to 30 minutes; The product obtained by cathodic electrodeposition was washed with deionized water until neutral and then dried overnight under vacuum to obtain E-Pb@C.

6. The method for preparing a bimetallic lead-silver catalyst according to claim 1, characterized in that, In step S3, The silver salt is selected from one of silver nitrate, silver fluoroborate, and silver perchlorate; The concentration of the silver salt is 1-50 mmol / L; The molar ratio of silver salt to lead salt is 0 to 4:1, and is not 0.

7. The method for preparing a bimetallic lead-silver catalyst according to claim 1, characterized in that, In step S3, The conditions for the in-situ exchange reaction are as follows: The temperature is 25℃, and the time is 2~30 minutes; The product obtained from the in-situ substitution reaction was washed with deionized water until neutral and then dried under vacuum overnight to obtain the E-PbAg@C catalyst.

8. A bimetallic lead-silver catalyst, characterized in that, It is prepared by any one of the preparation methods described in claims 1 to 7; The active metal component of the bimetallic lead-silver catalyst has a plate-like morphology.

9. The application of the bimetallic lead-silver catalyst as described in claim 8 in the electrocatalytic hydrogenation of levulinic acid to synthesize 4-hydroxyvalerate.

10. The application according to claim 9, characterized in that, The reaction conditions for the electrocatalytic hydrogenation are as follows: The temperature is 25℃ and the potential is -1.38 V. RHE .

Citation Information

Patent Citations

  • Catalyst for preparing gamma-valerolactone through electrochemical hydrogenation of levulinic acid as well as preparation and use methods of catalyst

    CN116536691A