Alloy material and preparation method thereof, mold
By preparing an alloy material containing tungsten carbide, a binder phase, tantalum carbide, chromium, and carbon compounds, the problem of wear and cracking of lithium battery tab molds in high-frequency, high-impact operations was solved, achieving wear resistance and extended lifespan of the mold, and ensuring production continuity and tab forming precision.
Patent Information
- Application Number
- CN202610901908.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-22
- Publication Date
- 2026-07-24
AI Technical Summary
Existing lithium battery tab molds are prone to wear, chipping, and fatigue cracks during high-frequency, high-impact tab stamping operations, affecting production continuity and tab forming accuracy.
An alloy material, including tungsten carbide, a binder phase, tantalum carbide, chromium, and carbon compounds, is used to prepare a mold by grinding, mixing, pressing, and sintering. The sintering temperature is 1350-1450℃, and the process is carried out under a protective atmosphere. Rare earth elements and oxides are added to enhance the bonding strength.
It improves the wear resistance and lifespan of the mold, reduces wear, chipping and fatigue cracks, and ensures production continuity and tab forming accuracy.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials technology, specifically relating to an alloy material, its preparation method, and a mold. Background Technology
[0002] Molds are common molds and tools in industrial production. They are used to create shaped parts or items and can be composed of various parts, with different molds consisting of different components. They are widely used in injection molding, powder metallurgy pressing, and casting. Molds have complex shapes and withstand the expansion forces of the blank during processing, requiring high structural strength, hardness, roughness, and precision. The development of mold production has a significant impact on the manufacturing of mechanical parts or products. In the preparation of lithium battery tabs, molds are required. Currently, lithium battery tab molds are mostly made of hard alloy materials, with a common formulation being a composite system of tungsten carbide (WC) and cobalt (Co). The main preparation method is powder metallurgy, where the raw materials are mixed, pressed, and then sintered. Although this type of material has a certain degree of wear resistance, it is still prone to wear, chipping, and fatigue cracks in high-frequency, high-impact tab stamping operations, leading to insufficient mold life and affecting production continuity and tab forming accuracy. Summary of the Invention
[0003] The purpose of this invention is to provide an alloy material, its preparation method, and a mold to solve the problem of poor performance of lithium battery tab molds.
[0004] In a first aspect, embodiments of the present invention provide an alloy material, comprising: Tungsten carbide; binder phase; Tantalum carbide; chromium; Carbon compounds, said carbon compounds including at least one of titanium carbide, niobium carbide and vanadium carbide.
[0005] Optionally, the alloy material includes: 85-92 parts by weight of tungsten carbide; 5-8 parts by weight of binder phase; 0.3-1.5 parts by weight of tantalum carbide; Chromium 0.2-1 parts by weight; The carbon compound includes at least one of titanium carbide, niobium carbide, and vanadium carbide, and the carbon compound is present in 0.5-2 parts by weight.
[0006] Optionally, the binder phase comprises: At least one of cobalt, cobalt-nickel alloy, and cobalt-iron alloy.
[0007] Optionally, the alloy material further includes: Rare earth elements: 0.05-0.3 parts by weight.
[0008] Optionally, the rare earth elements include: At least one of yttrium, lanthanum, scandium, and cerium.
[0009] Optionally, it also includes: Zirconium oxide, boron oxide, carbon, zirconium, boron, barium carbonate; Zirconium oxide is 0.4-1 parts by weight, boron oxide is 0.4-1.2 parts by weight, carbon is 0.8-2 parts by weight, zirconium is 0.3-0.8 parts by weight, boron is 0.3-0.7 parts by weight, and barium carbonate is 0.3-0.6 parts by weight.
[0010] Secondly, embodiments of the present invention provide a method for preparing an alloy material, comprising: The raw materials are ground and mixed to obtain a mixed powder; the raw materials include: tungsten carbide; binder phase; tantalum carbide; chromium; carbon compound, wherein the carbon compound includes at least one of titanium carbide, niobium carbide and vanadium carbide; The mixed powder is placed in a mold and pressed into shape to obtain a green part; The green parts are sintered; After sintering and cooling, an alloy material is obtained.
[0011] Optionally, the step of sintering the green part includes: The green parts are sintered under a vacuum or inert gas atmosphere; and / or the sintering temperature is 1350-1450℃, and the sintering holding time is 60-120min.
[0012] Optionally, the raw materials include: 85-92 parts by weight of tungsten carbide; 5-8 parts by weight of binder phase; 0.3-1.5 parts by weight of tantalum carbide; Chromium 0.2-1 parts by weight; 0.5-2 parts by weight of carbon compounds.
[0013] Optionally, the binder phase comprises: At least one of cobalt, cobalt-nickel alloy, and cobalt-iron alloy; and / or The alloy material also includes: 0.05-0.3 parts by weight of rare earth elements.
[0014] Optionally, the raw materials further include: Zirconium oxide, boron oxide, carbon, zirconium, boron, barium carbonate; The steps of sintering the green parts include: First, place the green blank in a vacuum and sinter it at 1050-1300℃ for 1-3 hours; Then place it in the first atmosphere and sinter at 1350-1450℃ for 1-2 hours; Then it is placed in a second atmosphere and sintered at 1120-1250℃ for 1-2.5h; The first atmosphere is nitrogen, and the second atmosphere is a mixture of methane and nitrogen. Zirconium oxide 0.4-1 parts by weight, boron oxide 0.4-1.2 parts by weight, carbon 0.8-2 parts by weight, zirconium 0.3-0.8 parts by weight, boron 0.3-0.7 parts by weight, barium carbonate 0.3-0.6 parts by weight.
[0015] Thirdly, embodiments of the present invention provide a lithium battery tab mold, which is prepared using the alloy material described in the above embodiments, or using the alloy material prepared by the preparation method described in the above embodiments.
[0016] The alloy material of this invention includes: tungsten carbide; a binder phase; tantalum carbide; chromium; and a carbon compound, wherein the carbon compound includes at least one of titanium carbide, niobium carbide, and vanadium carbide. The mold prepared using the above alloy material can be used to manufacture lithium battery tabs. This material has good wear resistance and is not prone to wear, chipping, fatigue cracks, etc., during high-frequency, high-impact tab stamping operations. The mold has a long lifespan and does not affect production continuity or tab forming accuracy. Detailed Implementation
[0017] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] The alloy material of this invention includes: Tungsten carbide; binder phase; tantalum carbide; chromium; carbon compound, wherein the carbon compound includes at least one of titanium carbide, niobium carbide, and vanadium carbide. The alloy material for lithium battery tab molds in this embodiment of the invention, through which a mold prepared using the above alloy material can be used to manufacture lithium battery tabs, exhibits good wear resistance and is not prone to wear, chipping, fatigue cracks, etc., during high-frequency, high-impact tab stamping operations. The mold has a long lifespan and does not affect production continuity or tab forming accuracy.
[0019] In some embodiments, the alloy material may include: The alloy comprises: 85-92 parts by weight of tungsten carbide; 5-8 parts by weight of binder phase; 0.3-1.5 parts by weight of tantalum carbide; 0.2-1 parts by weight of chromium; and a carbon compound, wherein the carbon compound includes at least one of titanium carbide, niobium carbide, and vanadium carbide, and the carbon compound is 0.5-2 parts by weight. For example, the alloy material may include: 85 parts by weight of tungsten carbide; 5 parts by weight of binder phase; 1.5 parts by weight of tantalum carbide; 0.2 parts by weight of chromium; and a carbon compound, wherein the carbon compound includes titanium carbide, and the titanium carbide is 0.5 parts by weight. Alternatively, the alloy material may include: 92 parts by weight of tungsten carbide; 7 parts by weight of binder phase; 1 part by weight of tantalum carbide; 0.7 parts by weight of chromium; and a carbon compound, wherein the carbon compound includes titanium carbide, and the titanium carbide is 1 part by weight.
[0020] In some embodiments, the binder phase may include: At least one of cobalt, cobalt-nickel alloy, and cobalt-iron alloy. For example, the binder phase may be cobalt, cobalt-nickel alloy, or cobalt-iron alloy, or a mixture of cobalt and cobalt-nickel alloy.
[0021] Optionally, the alloy material may further include: Rare earth elements are present in 0.05-0.3 parts by weight. For example, rare earth elements can be present in 0.05, 0.1, 0.2 or 0.3 parts by weight.
[0022] Optionally, the rare earth element may include: At least one of yttrium, lanthanum, scandium, and cerium. For example, rare earth elements may include yttrium, lanthanum, scandium, or cerium, and rare earth elements may include yttrium and lanthanum. The addition of rare earth elements can refine grains and enhance interfacial bonding strength.
[0023] In some embodiments, the alloy material further includes: Zirconia, boron oxide, carbon, zirconium, boron, and barium carbonate, with zirconium oxide at 0.4-1 parts by weight, boron oxide at 0.4-1.2 parts by weight, carbon at 0.8-2 parts by weight, zirconium at 0.3-0.8 parts by weight, boron at 0.3-0.7 parts by weight, and barium carbonate at 0.3-0.6 parts by weight.
[0024] The method for preparing the alloy material according to embodiments of the present invention includes: The raw materials are ground and mixed to obtain a mixed powder; the raw materials include: tungsten carbide; binder phase; tantalum carbide; chromium; carbon compound, wherein the carbon compound includes at least one of titanium carbide, niobium carbide and vanadium carbide; The mixed powder is placed in a mold and pressed into shape to obtain a green part; The green parts are sintered, for example, at a sintering temperature of 1350-1450℃ and a sintering holding time of 60-120min; After sintering and cooling, an alloy material is obtained.
[0025] The alloy material prepared by the above method and components can be used to prepare molds, which can be used to prepare lithium battery tabs. The material has good wear resistance and is not prone to wear, chipping, fatigue cracks, etc. in high-frequency, high-impact tab stamping operations. The mold has a long life and does not affect the continuity of production or the forming accuracy of the tabs.
[0026] Optionally, the step of sintering the green part includes: The green parts are sintered under a vacuum or inert gas atmosphere. The inert gas atmosphere can be nitrogen.
[0027] Optionally, the alloy material includes: Tungsten carbide 85-92 parts by weight; binder phase 5-8 parts by weight; tantalum carbide 0.3-1.5 parts by weight; Chromium 0.2-1 parts by weight; carbon compound, said carbon compound including at least one of titanium carbide, niobium carbide and vanadium carbide, the carbon compound being 0.5-2 parts by weight.
[0028] Optionally, the binder phase comprises: At least one of cobalt, cobalt-nickel alloy, and cobalt-iron alloy. For example, the binder phase may be cobalt, cobalt-nickel alloy, or cobalt-iron alloy, or a mixture of cobalt and cobalt-nickel alloy.
[0029] Optionally, the alloy material further includes: Rare earth elements are present in amounts of 0.05-0.3 parts by weight. For example, rare earth elements can be present in amounts of 0.05, 0.1, 0.2, or 0.3 parts by weight.
[0030] Optionally, the rare earth element includes at least one of yttrium, lanthanum, scandium, and cerium. For example, the rare earth element may include yttrium, lanthanum, scandium, or cerium, and the rare earth element may include yttrium or lanthanum.
[0031] In some embodiments, the raw materials may further include: Zirconium oxide, boron oxide, carbon, zirconium, boron, barium carbonate; The step of sintering the green part may include: First, place the green blank in a vacuum and sinter it at 1050-1300℃ for 1-3 hours; Then place it in the first atmosphere and sinter at 1350-1450℃ for 1-2 hours; Then it is placed in a second atmosphere and sintered at 1120-1250℃ for 1-2.5h; The first atmosphere is nitrogen, and the second atmosphere is a mixture of methane and nitrogen; the volume of methane in the methane-nitrogen mixture is 5-12%. Zirconium oxide 0.4-1 parts by weight, boron oxide 0.4-1.2 parts by weight, carbon 0.8-2 parts by weight, zirconium 0.3-0.8 parts by weight, boron 0.3-0.7 parts by weight, barium carbonate 0.3-0.6 parts by weight.
[0032] The lithium battery tab mold of this invention is prepared using the alloy material described in the above embodiments, or using the alloy material prepared by the preparation method described in the above embodiments.
[0033] The present invention will be further described below through some specific embodiments.
[0034] Example 1: A method for preparing alloy materials for lithium battery tab molds, including the following steps: The raw materials are ground and mixed to obtain a mixed powder; the raw materials include: tungsten carbide; binder phase; tantalum carbide; chromium; carbon compound, wherein the carbon compound is titanium carbide; The mixed powder is placed in a mold and pressed into shape to obtain a green part; The green parts are sintered in a vacuum or inert gas atmosphere at a temperature of 1350℃ for 120 minutes. After sintering and cooling, an alloy material is obtained; The raw materials include: 85 parts by weight of tungsten carbide; 8 parts by weight of cobalt binder phase; 0.3 parts by weight of tantalum carbide; 0.2 parts by weight of chromium; and 2 parts by weight of carbon compounds.
[0035] Example 2: A method for preparing alloy materials for lithium battery tab molds, including the following steps: The raw materials are ground and mixed to obtain a mixed powder; the raw materials include: tungsten carbide; binder phase; tantalum carbide; chromium; carbon compound, wherein the carbon compound is titanium carbide; The mixed powder is placed in a mold and pressed into shape to obtain a green part; The green parts are sintered in a vacuum or inert gas atmosphere at a temperature of 1450℃ for 60 minutes. After sintering and cooling, an alloy material is obtained; The raw materials include: 92 parts by weight of tungsten carbide; 5 parts by weight of cobalt binder phase; 1.5 parts by weight of tantalum carbide; 1 part by weight of chromium; and 0.5 parts by weight of carbon compounds.
[0036] Example 3: A method for preparing alloy materials for lithium battery tab molds, including the following steps: The raw materials are ground and mixed to obtain a mixed powder; the raw materials include: tungsten carbide; binder phase; tantalum carbide; chromium; carbon compound, wherein the carbon compound is titanium carbide; The mixed powder is placed in a mold and pressed into shape to obtain a green part; The green parts are sintered in a vacuum or inert gas atmosphere at a temperature of 1400℃ for 90 minutes. After sintering and cooling, an alloy material is obtained; The raw materials include: 89 parts by weight of tungsten carbide; 7 parts by weight of cobalt binder phase; 1 part by weight of tantalum carbide; 0.7 parts by weight of chromium; and 1.2 parts by weight of carbon compounds.
[0037] Example 4: The difference between Example 4 and Example 3 is as follows: The raw materials contain 0.05-0.3 parts by weight of rare earth elements, including yttrium and lanthanum, with a mass ratio of yttrium to lanthanum of 2:1.
[0038] Example 5: The difference between Example 5 and Example 3 is as follows: The raw materials also include: Zirconium oxide, boron oxide, carbon, zirconium, boron, barium carbonate; The steps of sintering the green parts include: First, place the green blank in a vacuum and sinter it at 1050℃ for 3 hours; Then place it in the first atmosphere and sinter at 1450℃ for 1 hour; Then it was placed in a second atmosphere and sintered at 1120℃ for 2.5h; The first atmosphere is nitrogen, and the second atmosphere is a mixture of methane and nitrogen; the volume of methane in the methane-nitrogen mixture is 5%. Zirconium oxide 0.4 parts by weight, boron oxide 1.2 parts by weight, carbon 0.8 parts by weight, zirconium 0.3 parts by weight, boron 0.7 parts by weight, barium carbonate 0.3 parts by weight.
[0039] Example 6: The difference between Example 6 and Example 3 is as follows: The raw materials also include: Zirconium oxide, boron oxide, carbon, zirconium, boron, barium carbonate; The steps of sintering the green parts include: First, place the green blank in a vacuum and sinter it at 1300℃ for 1 hour; Then place it in the first atmosphere and sinter at 1350℃ for 2 hours; Then it was placed in a second atmosphere and sintered at 1250℃ for 1 hour; The first atmosphere is nitrogen, and the second atmosphere is a mixture of methane and nitrogen; the volume of methane in the methane-nitrogen mixture is 12%. Zirconium oxide 1 part by weight, boron oxide 0.4 parts by weight, carbon 2 parts by weight, zirconium 0.8 parts by weight, boron 0.3 parts by weight, barium carbonate 0.6 parts by weight.
[0040] Comparative Example 1: The difference between Comparative Example 1 and Example 6 is as follows: Both the first and second atmospheres are replaced with vacuum.
[0041] Comparative Example 2: The difference between Comparative Example 2 and Example 6 is as follows: The second atmosphere was replaced with nitrogen.
[0042] The mold was prepared using the alloy material in the above embodiments, and the performance of the mold was tested. The specific test results are shown in Table 1.
[0043] Table 1 Performance test results of the mold ; As shown in Table 1, the molds prepared from the materials in the above embodiments have good wear resistance, significantly extended mold service life, high impact resistance, reduced risk of chipping and cracking, and are suitable for continuous high-speed stamping.
[0044] The mold of the alloy material prepared above was placed in a 1.5 mol / L sulfuric acid solution at 40°C for 72 h, and then placed in a 1.5 mol / L sodium hydroxide solution at 40°C for 72 h. The performance of the mold was tested, and the specific test results are shown in Table 2.
[0045] Table 2 Performance test results of the mold ; As shown in Table 2, the molds prepared from the materials in the above embodiments have good acid and alkali resistance. Their performance remains basically unchanged after treatment in acidic or alkaline solutions, which can meet the requirements for use in battery tab molds.
[0046] The embodiments of the present invention have been described above, but the present invention is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of the present invention without departing from the spirit and scope of the claims, and all of these forms are within the protection scope of the present invention.
Claims
1. An alloy material, characterized in that, include: Tungsten carbide; binder phase; Tantalum carbide; chromium; Carbon compounds, said carbon compounds including at least one of titanium carbide, niobium carbide and vanadium carbide.
2. The alloy material according to claim 1, characterized in that, The alloy material includes: 85-92 parts by weight of tungsten carbide; 5-8 parts by weight of binder phase; 0.3-1.5 parts by weight of tantalum carbide; Chromium 0.2-1 parts by weight; The carbon compound includes at least one of titanium carbide, niobium carbide, and vanadium carbide, and the carbon compound is present in 0.5-2 parts by weight.
3. The alloy material according to claim 1, characterized in that, The binder phase includes: At least one of cobalt, cobalt-nickel alloy, and cobalt-iron alloy; and / or Rare earth elements: 0.05-0.3 parts by weight.
4. The alloy material according to claim 1, characterized in that, Also includes: Zirconium oxide, boron oxide, carbon, zirconium, boron, barium carbonate; Zirconium oxide is 0.4-1 parts by weight, boron oxide is 0.4-1.2 parts by weight, carbon is 0.8-2 parts by weight, zirconium is 0.3-0.8 parts by weight, boron is 0.3-0.7 parts by weight, and barium carbonate is 0.3-0.6 parts by weight.
5. A method for preparing an alloy material, characterized in that, include: The raw materials are ground and mixed to obtain a mixed powder; the raw materials include: tungsten carbide; binder phase; tantalum carbide; chromium; carbon compound, wherein the carbon compound includes at least one of titanium carbide, niobium carbide and vanadium carbide; The mixed powder is placed in a mold and pressed into shape to obtain a green part; The green parts are sintered; After sintering and cooling, an alloy material is obtained.
6. The preparation method according to claim 5, characterized in that, The steps of sintering the green blanks include: sintering the green blanks under a vacuum or inert gas atmosphere; and / or The sintering temperature is 1350-1450℃, and the sintering holding time is 60-120min.
7. The preparation method according to claim 5, characterized in that, The raw materials include: 85-92 parts by weight of tungsten carbide; 5-8 parts by weight of binder phase; 0.3-1.5 parts by weight of tantalum carbide; Chromium 0.2-1 parts by weight; 0.5-2 parts by weight of carbon compounds.
8. The preparation method according to claim 7, characterized in that, The binder phase includes: At least one of cobalt, cobalt-nickel alloy, and cobalt-iron alloy; and / or The alloy material also includes: 0.05-0.3 parts by weight of rare earth elements.
9. The preparation method according to claim 8, characterized in that, The raw materials also include: Zirconium oxide, boron oxide, carbon, zirconium, boron, barium carbonate; The steps of sintering the green parts include: First, place the green blank in a vacuum and sinter it at 1050-1300℃ for 1-3 hours; Then place it in the first atmosphere and sinter at 1350-1450℃ for 1-2 hours; Then it is placed in a second atmosphere and sintered at 1120-1250℃ for 1-2.5h; The first atmosphere is nitrogen, and the second atmosphere is a mixture of methane and nitrogen. Zirconium oxide 0.4-1 parts by weight, boron oxide 0.4-1.2 parts by weight, carbon 0.8-2 parts by weight, zirconium 0.3-0.8 parts by weight, boron 0.3-0.7 parts by weight, barium carbonate 0.3-0.6 parts by weight.
10. A lithium battery tab mold, characterized in that, The alloy material prepared using any one of claims 1-4, or the alloy material prepared using any one of claims 5-9.